A modified polysulfone porous membrane and its preparation method and application

By depositing a titanium dioxide layer on the polyphenylsulfone porous membrane substrate and performing photocatalytic modification, the problem of reduced hydrophilicity caused by nanoparticles is solved, and the water vapor transmission performance and service life of the fuel cell humidifier are improved.

CN117965027BActive Publication Date: 2024-11-01GRINM RESOURCES & ENVIRONMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410193589.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-11-01
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

After long-term use of the existing polyphenylsulfone porous membrane, the titanium dioxide nanoparticles are prone to fall off, resulting in a decrease in hydrophilicity and a decrease in water vapor permeability efficiency, which affects the humidity enhancement performance and product life of fuel cell humidifiers.

Method used

Polysulfone-like porous membrane substrate with a spongy loose structure was prepared by non-solvent phase separation technology, and atomic deposition technology was used to deposit titanium dioxide layer on its surface, combined with photocatalytic methods for hydrophilic modification, using nano-silicon emulsion or allyl groups Glycidyl ether acts as a modifier to improve the hydrophilicity and stability of the membrane.

Benefits of technology

It significantly improves the hydrophilicity and stability of the membrane, extends the service life, maintains high mechanical strength and porous characteristics, improves water vapor transmission efficiency, and enhances the performance of fuel cell humidifiers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117965027B_ABST
    Figure CN117965027B_ABST
Patent Text Reader

Abstract

The present invention provides a modified polysulfone porous membrane and a preparation method and application thereof, which is prepared by combining atomic deposition with a photocatalytic method, and optimizing the vacuum degree of the atomic deposition equipment, the type and content of the surface modifier, and constructing a modified titanium dioxide layer on the surface of the polysulfone porous membrane substrate. The modified polysulfone porous membrane has a porosity of 40-70%, a tensile strength of 5-20 MPa, an elongation at break of 10-70%, a water contact angle of 10-30°, a water vapor / air selectivity of greater than 1100, and a water vapor permeability of 0.14 g·min ‑1 cm ‑2 MPa ‑1 It not only retains the high mechanical strength and porous characteristics of the polysulfone porous membrane substrate, but also significantly improves the hydrophilicity and stability of the membrane, can improve the membrane humidification efficiency, can be applied to fuel cell membrane humidifiers, and increase the service life of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cells, and in particular to a modified polysulfone porous membrane and a preparation method and application thereof. Background Art

[0002] As a new type of energy conversion equipment, fuel cells are highly efficient and environmentally friendly, and the intake humidification of fuel cells is an important process, which has a significant impact on the performance and life of fuel cells. Intake humidification refers to the humidification of hydrogen and oxygen entering the fuel cell in the fuel cell system to improve the efficiency and stability of the fuel cell. The working principle of the fuel cell is to generate electricity through the electrochemical reaction of hydrogen and oxygen. This reaction needs to be carried out under certain stability and humidity conditions. Therefore, proper humidity is crucial to the normal operation of the fuel cell.

[0003] Hydrophilic porous membranes have pores of a size that can separate gases, and among various inorganic membranes, they have excellent gas separation properties, can be used in environments that require heat resistance and chemical resistance, and are low-cost. For this reason, hydrophilic porous membranes have been widely used in fuel cell humidifiers in recent years.

[0004] In order to improve the hydrophilicity of the porous membrane, some scholars directly mixed titanium dioxide into the polyphenylsulfone mixed matrix membrane for the preparation of hydrophilic porous membrane. The hydrophilicity of the polyphenylsulfone mixed matrix membrane was improved by this method, and the polyphenylsulfone porous hydrophilic membrane obtained by the treatment had the following problems: after the polyphenylsulfone porous hydrophilic membrane was operated for a long time, the titanium dioxide nanoparticles blended in the polyphenylsulfone mixed matrix membrane were easy to fall off, resulting in a decrease in the hydrophilicity of the polyphenylsulfone porous membrane and a decrease in the water vapor permeation efficiency, which further caused a decrease in the humidification performance of the fuel cell humidifier, thereby affecting the product life. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention provides a modified polysulfone porous membrane and a preparation method and application thereof, wherein a polysulfone porous membrane substrate having a sponge-like loose structure is prepared by a non-solvent induced phase separation technique, and a titanium dioxide layer is deposited on the surface of the polysulfone porous membrane substrate by an atomic deposition technique, and then the obtained modified polysulfone porous membrane precursor with a titanium dioxide layer deposited on the surface is hydrophilically modified with a modifier, and the modified polysulfone porous membrane is obtained by photocatalysis, washing and drying. The modified polysulfone porous membrane retains the high mechanical strength and porous characteristics of the polysulfone porous membrane substrate, and also significantly improves the hydrophilicity and stability of the membrane, can improve the membrane humidification efficiency, and greatly increases the service life of the membrane.

[0006] The specific content of the invention is as follows:

[0007] In a first aspect, the present invention provides a modified polysulfone porous membrane, wherein the modified polysulfone porous membrane is composed of a polysulfone porous membrane substrate and a modified titanium dioxide layer;

[0008] Wherein, the polysulfone porous membrane substrate is a sponge-like loose structure;

[0009] The polysulfone material constituting the polysulfone porous membrane substrate is one or more of polyethersulfone, polyphenylsulfone, polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone and sulfonated polysulfone.

[0010] Optionally, the polysulfone porous membrane has a porosity of 40-70%, a tensile strength of 5-20 MPa, an elongation at break of 10-70%, and a water contact angle of 10-30°.

[0011] In a second aspect, the present invention provides a method for preparing the modified polysulfone porous membrane according to the first aspect, the preparation method comprising:

[0012] Step 1, placing a polysulfone porous membrane substrate in an atomic layer deposition equipment reaction chamber at a temperature of 50-200° C. and a vacuum degree of 0-15 mbar, introducing a gaseous titanium-containing precursor into the reaction chamber for 100-1000 milliseconds, introducing an inert gas at a flow rate of 10-300 sccm for purging for 10-200 seconds, introducing a gaseous oxygen-containing precursor for 10-500 milliseconds, and finally introducing the inert gas at a flow rate of 10-300 sccm for a second purge for 10-200 seconds to complete the first deposition of titanium dioxide on the polysulfone porous membrane substrate;

[0013] Step 2, repeating step 1 to complete 10-500 depositions to obtain a modified polysulfone porous membrane precursor with a titanium dioxide layer deposited on the surface;

[0014] Step 3, spraying a modifier onto the surface of the modified polysulfone porous membrane precursor, and irradiating the modified polysulfone porous membrane precursor with a 100-1000 joule xenon lamp for 1-300 minutes to hydrophilically modify the modified polysulfone porous membrane precursor, and washing and drying to obtain the modified polysulfone porous membrane;

[0015] Wherein, the modifier is any one of nano-silicon emulsion and allyl glycidyl ether.

[0016] Optionally, the titanium-containing precursor is any one of titanium alkoxide, titanium halide and titanium alkylphthalamide.

[0017] Optionally, the oxygen-containing precursor is O 3 , H 2 O and H 2 O 2 Any of .

[0018] Optionally, the inert gas is Ar and N2 Any of .

[0019] Optionally, the modifier is 0.1-10 wt % of allyl glycidyl ether.

[0020] Optionally, the method for preparing the polysulfone porous membrane substrate comprises:

[0021] The polysulfone material, the solvent and the additive are uniformly mixed in a mass ratio of 14-35:52-85.9:0.1-34, and stirred for 4 hours at a temperature of 50-150° C. and a stirring speed of 200-300 r / min to obtain a casting liquid; the solvent is mixed with water to obtain a core liquid;

[0022] Injecting the core liquid and the casting liquid into a spinneret, extruding the casting liquid through the spinneret, and after an air process, immersing the casting liquid in a water coagulation bath at room temperature for solidification and forming, thereby obtaining the polysulfone porous membrane substrate;

[0023] The solvent is one or more of dichloromethane, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, carbon tetrachloride, N-methylpyrrolidone, methanol, ethanol and diethylene glycol;

[0024] The additive is one or more of sodium lauryl sulfate, suberic acid, oxalic acid, polyvinyl pyrrolidone, dibenzylidene sorbitol and benzoic acid.

[0025] Optionally, the polysulfone material is one or more of polyethersulfone, polyphenylsulfone, polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone and sulfonated polysulfone.

[0026] In a third aspect, the present invention provides a use of the modified polysulfone porous membrane described in the first aspect or the modified polysulfone porous membrane prepared by the preparation method described in the second aspect in a fuel cell membrane humidifier.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] (1) The present invention provides a modified polysulfone porous membrane, which is prepared by constructing a modified titanium dioxide layer on the surface of a polysulfone porous membrane substrate by combining atomic deposition and photocatalysis. The modified polysulfone porous membrane has a porosity of 40-70%, a tensile strength of 5-20 MPa, an elongation at break of 10-70%, a water contact angle of 10-30°, a water vapor / air selectivity of greater than 1100, and a water vapor permeability of 0.14 g·min -1 cm -2 MPa -1It not only retains the high mechanical strength and porous characteristics of the polysulfone porous membrane substrate, but also significantly improves the hydrophilicity and stability of the membrane, can improve the membrane humidification efficiency, and greatly increase the membrane service life.

[0029] The present invention provides a method for preparing a modified polysulfone porous membrane, which preferably selects the vacuum degree of the atomic deposition equipment, the type and content of the surface modifier, and utilizes the atomic deposition method to enable the titanium dioxide layer to be uniformly deposited on the surface of the polysulfone porous membrane substrate with a high specific surface area. Compared with directly coating titanium dioxide nanoparticles on the surface of the polysulfone porous membrane or adding titanium dioxide nanoparticles to the polysulfone porous membrane liquid, the titanium dioxide layer deposited on the surface of the polysulfone porous membrane by the atomic deposition technology of the present invention is more solid, and the titanium dioxide layer on the surface of the modified polysulfone porous membrane is not easy to fall off during the water vapor permeation process. After running for 100 hours, it still maintains a good hydrophilic effect and water vapor permeability, and the service life of the modified polysulfone porous membrane is greatly increased. In addition, the present invention specifically selects allyl glycidyl ether with high surface energy and low cost as a surface modifier, and uses a photocatalytic method to treat the polysulfone polymer / TiO 2 The surface of the formed porous membrane is coated, and the hydrophilicity of the membrane is improved on the basis of maintaining the porosity of the original membrane, thereby improving the water vapor permeability of the modified membrane. The preparation method is simple in procedure, easy to operate, controllable and easy to scale up, and has a very high application prospect in the field of preparation of fuel cell membrane humidifier materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 The flowchart of the preparation method of the modified polysulfone porous membrane provided by the embodiment of the present invention is shown;

[0032] Figure 2 The SEM image of the membrane cross section of the modified polyphenylsulfone porous membrane 1 provided in Example 1 of the present invention is shown;

[0033] Figure 3 The contact angle image of the modified polyphenylsulfone porous membrane 1 provided in Example 1 of the present invention is shown;

[0034] Figure 4 The membrane cross-section SEM image of the polyphenylsulfone porous membrane substrate provided in Comparative Example 1 of the present invention is shown;

[0035] Figure 5The contact angle image of the polyphenylsulfone porous membrane substrate provided in Comparative Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present invention and its application or use. Based on the embodiments of the present invention, any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts falls within the scope of protection of the present invention. In addition, all other embodiments obtained by ordinary technicians in this field without carrying out creative work belong to the scope of protection of the present invention.

[0037] In the embodiment, no specific experimental steps or conditions are indicated, and the operation or conditions of the conventional experimental steps described in the prior art in this field can be carried out. The reagents used and other instruments that do not indicate the manufacturer are conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.

[0038] Technologies, methods, and apparatus known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, such technologies, methods, and apparatus should be considered part of the authorization specification.

[0039] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0040] In the prior art, when preparing a membrane humidifier in a proton exchange membrane fuel cell, in order to improve the hydrophilicity of the membrane, titanium dioxide nanoparticles are usually directly mixed into a polysulfone mixed matrix membrane for the preparation of a hydrophilic porous membrane. However, there are problems such as the titanium dioxide nanoparticles being easy to fall off, the membrane having low mechanical strength, poor stability, short service life, and low hydrophilicity, making it difficult to use it for a long time, and being unable to achieve the desired membrane humidification efficiency and durability. Against this background, the present invention, after repeated analysis and demonstration, literature review and combined with experimental exploration, first prepares a polysulfone porous membrane substrate with a sponge pore structure to promote the deposition of a titanium dioxide layer, and then adopts a combination of atomic deposition technology and a photocatalytic method to prepare a humidification membrane. Specifically, a polysulfone porous membrane substrate with a sponge-like loose structure is prepared by a non-solvent induced phase separation technique, and a titanium dioxide layer is deposited on the surface of the polysulfone porous membrane substrate by an atomic deposition technique. The surface of the modified polysulfone porous membrane with a titanium dioxide layer deposited on the surface is then sprayed with a modifier for hydrophilic modification. After photocatalysis, washing and drying, a modified polysulfone porous membrane with high mechanical strength, porous properties, excellent membrane hydrophilicity, high water vapor permeability and stability is obtained to solve the above-mentioned problems existing in the prior art.

[0041] The specific implementation methods are as follows:

[0042] In a first aspect, the present invention provides a modified polysulfone porous membrane, wherein the modified polysulfone porous membrane is composed of a polysulfone porous membrane substrate and a modified titanium dioxide layer;

[0043] Wherein, the polysulfone porous membrane substrate is a sponge-like loose structure;

[0044] The polysulfone material constituting the polysulfone porous membrane substrate is one or more of polyethersulfone, polyphenylsulfone, polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone and sulfonated polysulfone.

[0045] In some embodiments, the polysulfone porous membrane has a porosity of 40-70%, a tensile strength of 5-20 MPa, an elongation at break of 10-70%, a water contact angle of 10-30°, and a service life of more than 100 h.

[0046] In a second aspect, the present invention provides a method for preparing the modified polysulfone porous membrane described in the first aspect. Figure 1 The flow chart of the preparation method of the modified polysulfone porous membrane provided in the embodiment of the present invention is shown as follows: Figure 1 As shown, the preparation method comprises:

[0047] Step 1, place a polysulfone porous membrane substrate in an atomic layer deposition equipment reaction chamber with a temperature of 50-200°C and a vacuum degree of 0-15 mbar, introduce a gaseous titanium-containing precursor into the reaction chamber for 100-1000 milliseconds, introduce an inert gas with a flow rate of 10-300 sccm for purging for 10-200 seconds, introduce a gaseous oxygen-containing precursor for 10-500 milliseconds, and finally introduce the inert gas with a flow rate of 10-300 sccm for a second purge for 10-200 seconds to complete the first deposition of titanium dioxide on the polysulfone porous membrane substrate.

[0048] When this step is implemented, a polysulfone porous membrane substrate with a sponge-like loose structure is first prepared by a non-solvent phase separation technology. Specifically, the polysulfone material, solvent, and additive are evenly mixed in a mass ratio of 14-35:52-85.9:0.1-34, stirred for 4 hours at a temperature of 50-150°C and a stirring speed of 200-300r / min, and then allowed to stand for degassing to obtain a casting liquid; the solvent is mixed with water to obtain a core liquid. The solvent is one or more of dichloromethane, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, carbon tetrachloride, N-methylpyrrolidone, methanol, ethanol, and diethylene glycol; the additive is one or more of sodium dodecyl sulfate, suberic acid, oxalic acid, polyvinylpyrrolidone, dibenzylidene sorbitol, and benzoic acid. The polysulfone material is one or more of polyethersulfone, polyphenylsulfone, polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone, and sulfonated polysulfone.

[0049] The casting liquid and the core liquid are respectively injected into the hollow fiber spinning machine through the casting liquid channel and the core liquid channel, and the casting liquid is extruded through the hollow spinneret, passed through the air process, and immersed in a water coagulation bath at room temperature for solidification and molding to obtain the polysulfone porous membrane substrate.

[0050] The polysulfone porous membrane substrate is placed in an atomic deposition equipment reaction chamber at a temperature of 50-200°C and a vacuum degree of 0-15 mbar, and a gaseous titanium-containing precursor is introduced into the reaction chamber for 100-1000 milliseconds, and then an inert gas with a flow rate of 10-300 sccm is introduced for purging for 10-200 seconds. Then, a gaseous oxygen-containing precursor is introduced for 10-500 milliseconds, and finally the inert gas with a flow rate of 10-300 sccm is introduced for a second purge of 10-200 seconds to complete the first deposition of titanium dioxide on the polysulfone porous membrane substrate. The titanium-containing precursor is any one of titanium alkoxide, titanium halide and titanium alkylphthalamide; the inert gas is Ar and N 2 The introduction of inert gas enables the titanium dioxide layer to be stably deposited on the surface of the polysulfone porous membrane substrate.

[0051] Step 2: Repeat step 1 to complete 10 to 500 depositions to obtain a modified polysulfone porous membrane precursor with a titanium dioxide layer deposited on the surface.

[0052] When this step is implemented, step 1 is repeated. When 200-300 depositions are completed, the titanium dioxide layer can be stably and evenly deposited on the surface of the polysulfone porous membrane substrate to the greatest extent, and the cost is relatively low.

[0053] Step 3: spray a modifier onto the surface of the modified polysulfone porous membrane precursor, and irradiate the modified polysulfone porous membrane precursor with a 100-1000 joule xenon lamp for 1-300 minutes to hydrophilically modify the modified polysulfone porous membrane precursor, and obtain the modified polysulfone porous membrane after washing and drying.

[0054] When this step is specifically implemented, the surface modifier can be coated on the modified polysulfone porous membrane precursor by spraying or immersion. The modifier is any one of nano-silicon emulsion and allyl glycidyl ether, which can further improve the hydrophilicity of the product membrane. The modifier is preferably 0.1-10wt% allyl glycidyl ether. The titanium dioxide layer introduces epoxy groups through addition reaction with allyl glycidyl ether, which not only improves the surface activity but also increases the hydrophilicity.

[0055] Among them, when the modifier is 0.3wt% of allyl glycidyl ether, the titanium-containing precursor is titanium alkoxide, and the photocatalysis is carried out by irradiating a 500-joule xenon lamp for 30 minutes, the prepared modified polysulfone porous membrane not only retains the good mechanical strength and porosity of the original polysulfone base membrane, but also has high membrane stability and hydrophilicity, with a water contact angle as low as 21.12°, a water vapor / air selectivity of 1127, and a water vapor permeability of 0.14g·min -1 cm -2 MPa -1 , with a service life of more than 100h, it can achieve better membrane humidification efficiency and stability.

[0056] The present invention adopts a method combining atomic deposition and photocatalysis to prepare a modified polysulfone porous membrane to improve the stability, hydrophilicity and service life of the membrane through water vapor, while retaining the rigidity and porosity of the original polysulfone membrane substrate, thereby overcoming the defect that the polysulfone substrate basically does not react with any reagent at room temperature and is extremely difficult to modify.

[0057] The modification method provided by the present invention can be applied to many scenarios where the hydrophilicity and hydrophobicity of the membrane cannot be modified by conventional solution methods due to the stable physical and chemical properties of the high molecular polymer raw materials.

[0058] In a third aspect, the present invention provides a use of the modified polysulfone porous membrane described in the first aspect or the modified polysulfone porous membrane prepared by the preparation method described in the second aspect in a fuel cell membrane humidifier.

[0059] In order to make those skilled in the art understand the present invention more clearly, the modified polysulfone porous membrane and its preparation method and application described in the present invention are now described in detail through the following examples and test examples. Among them, the selected polysulfone material is polyphenylsulfone.

[0060] Example 1

[0061] In this embodiment, a titanium dioxide layer is deposited on the surface of a polyphenylsulfone porous membrane substrate by atomic deposition technology to obtain a modified polyphenylsulfone porous membrane precursor. Then, a modifier is sprayed on the surface of the modified polyphenylsulfone porous membrane precursor by photocatalysis to obtain a modified polyphenylsulfone porous membrane. The surface modifier is 0.3wt% of allyl glycidyl ether. Specifically, as follows:

[0062] Step 1. Weigh polyphenylsulfone, N-methylpyrrolidone and sodium dodecyl sulfate in a mass ratio of 17:73:10, add them into the reactor in turn and stir, heat to 50-150°C, stir at 200r / min for 4 hours, and then degas to obtain a casting liquid. Then mix N-methylpyrrolidone and water in a volume ratio of 50%, and transfer the mixed solution to the core liquid furnace of the hollow fiber spinning machine as the core liquid. Use the casting liquid as the raw material, use a hollow fiber spinning machine for spinning, extrude the casting liquid, undergo an air process, and immerse it in a water coagulation bath for solidification. Soak the preliminarily solidified membrane filaments in deionized water to remove residual N-methylpyrrolidone and sodium dodecyl sulfate to obtain a polyphenylsulfone porous membrane substrate.

[0063] Step 2: An atomic layer deposition apparatus (D100-4882, Chongqing Nuotu Technology Co., Ltd.) is used as an atomic deposition apparatus. The apparatus is completely sealed relative to the external environment. The amount of gaseous titanium-containing precursor and gaseous oxygen-containing precursor introduced can be controlled by controlling the running time of the program in the apparatus. The reaction chamber of the atomic deposition apparatus is evacuated to a vacuum degree of 0.5 mbar, a polyphenylsulfone porous membrane substrate is placed in the reaction chamber, and then the reaction chamber temperature is heated to 100° C.; gaseous titanium tetraisopropoxide is introduced into the reaction chamber for 400 milliseconds, and then N with a flow rate of 50 sccm is used. 2 The purge was performed for 30 seconds; then gaseous H 2 O for 100 ms and finally N with a flow rate of 50 sccm 2 Purge for 30 seconds to complete the first deposition of the titanium dioxide layer on the polyphenylsulfone porous membrane substrate;

[0064] Step 3, repeating step 2 to complete 300 depositions to obtain a modified polyphenylene sulfone porous membrane precursor with a titanium dioxide layer deposited on the surface;

[0065] Step 4: spray 0.3 wt % of allyl glycidyl ether onto the surface of the modified polyphenylsulfone porous membrane precursor, irradiate with a 500 joule xenon lamp for 30 minutes to hydrophilically modify the modified polyphenylsulfone porous membrane precursor, rinse with anhydrous ethanol, and dry in the shade to obtain a modified polyphenylsulfone porous membrane 1.

[0066] Figure 2 The membrane cross-section SEM image of the modified polyphenylsulfone porous membrane 1 provided in Example 1 is shown. As shown in the figure, the membrane cross-section has a sponge-like pore structure, and the measured membrane porosity is 48.94%, the tensile strength is 5.98 MPa, and the elongation at break is 19.86%.

[0067] Figure 3 The contact angle image of the modified polyphenylsulfone porous membrane 1 provided in Example 1 is shown. As shown in the figure, the contact angle of the modified polyphenylsulfone porous membrane 1 is small. After measurement, the contact angle is 21.12°, and the hydrophilicity is relatively excellent.

[0068] Example 2

[0069] In this embodiment, a titanium dioxide layer is deposited on the surface of a polyphenylsulfone porous membrane substrate using an atomic deposition technique to obtain a modified polyphenylsulfone porous membrane precursor. Then, a modifier is sprayed on the surface of the modified polyphenylsulfone porous membrane precursor by photocatalysis to obtain a modified polyphenylsulfone porous membrane. The modifier is a nano-silicon emulsion. Specifically, as follows:

[0070] Step 1. Weigh polyphenylsulfone, N-methylpyrrolidone and sodium dodecyl sulfate in a mass ratio of 17:73:10, add them into the reactor in turn and stir, heat to 50-150°C, stir at 200r / min for 4 hours, and then degas to obtain a casting liquid. Then mix N-methylpyrrolidone and water in a volume ratio of 50%, and transfer the mixed solution to the core liquid furnace of the hollow fiber spinning machine as the core liquid. Use the casting liquid as the raw material, use a hollow fiber spinning machine for spinning, extrude the casting liquid, undergo an air process, and immerse it in a water coagulation bath for solidification. Soak the preliminarily solidified membrane filaments in deionized water to remove residual N-methylpyrrolidone and sodium dodecyl sulfate to obtain a polyphenylsulfone porous membrane substrate.

[0071] Step 2: An atomic layer deposition apparatus (D100-4882, Chongqing Nuotu Technology Co., Ltd.) is used as an atomic deposition apparatus. The apparatus is completely sealed relative to the external environment. The amount of gaseous titanium-containing precursor and gaseous oxygen-containing precursor introduced can be controlled by controlling the running time of the program in the apparatus. The reaction chamber of the atomic deposition apparatus is evacuated to a vacuum degree of 0.5 mbar, a polyphenylsulfone porous membrane substrate is placed in the reaction chamber, and then the reaction chamber temperature is heated to 100° C.; gaseous titanium tetraisopropoxide is introduced into the reaction chamber for 400 milliseconds, and then N with a flow rate of 50 sccm is used. 2 Purge for 30 seconds; introduce gaseous H 2 O for 100 ms and finally N with a flow rate of 50 sccm 2 Purge for 30 seconds to complete the first deposition of the titanium dioxide layer on the polyphenylsulfone porous membrane substrate;

[0072] Step 3, repeating step 2 to complete 300 depositions to obtain a modified polyphenylene sulfone porous membrane precursor with a titanium dioxide layer deposited on the surface;

[0073] Step 4, spraying nano-silicon emulsion onto the surface of the modified polyphenylsulfone porous membrane precursor, irradiating the modified polyphenylsulfone porous membrane precursor with a 500 joule xenon lamp for 30 minutes to hydrophilically modify the modified polyphenylsulfone porous membrane precursor, rinsing with anhydrous ethanol, and drying in the shade to obtain a modified polyphenylsulfone porous membrane 2. According to measurement, the porosity of the modified polyphenylsulfone porous membrane 2 is 49.82%, the contact angle is 60.59°, the tensile strength is 5.83 MPa, and the elongation at break is 17.19%.

[0074] The cross-sectional SEM image and contact angle image of the modified polyphenylsulfone porous membrane 2 prepared in Example 2 of the present invention are respectively Figure 2 , Figure 3 Similar, no longer given here.

[0075] Example 3

[0076] In this embodiment, a titanium dioxide layer is deposited on the surface of a polyphenylsulfone porous membrane substrate by atomic deposition technology to obtain a modified polyphenylsulfone porous membrane precursor. Then, a modifier is sprayed on the surface of the modified polyphenylsulfone porous membrane precursor by photocatalysis to obtain a modified polyphenylsulfone porous membrane. The modifier is 3 wt % allyl glycidyl ether. Specifically, as follows:

[0077] Step 1. Weigh polyphenylsulfone, N-methylpyrrolidone and sodium dodecyl sulfate in a mass ratio of 18:72:10, add them to the reactor in turn and stir, heat to 50-150°C, stir at 200r / min for 4 hours, and then degas to obtain a casting liquid. Then mix N-methylpyrrolidone and water in a volume ratio of 50%, and transfer the mixed solution to the core liquid furnace of the hollow fiber spinning machine as the core liquid. Use the casting liquid as the raw material, use a hollow fiber spinning machine for spinning, extrude the casting liquid, undergo an air process, and immerse it in a water coagulation bath for solidification. Soak the initially solidified membrane filaments in deionized water to remove residual N-methylpyrrolidone and sodium dodecyl sulfate to obtain a polyphenylsulfone porous membrane substrate.

[0078] Step 2: Use an atomic layer deposition apparatus (D100-4882, Chongqing Nuotu Technology Co., Ltd.) as an atomic deposition apparatus. The apparatus is completely sealed relative to the external environment. By controlling the running time of the program in the apparatus, the amount of gaseous titanium-containing precursor and gaseous oxygen-containing precursor introduced can be controlled. The reaction chamber of the atomic deposition apparatus is evacuated to a vacuum degree of 0.5 mbar, a polysulfone porous membrane substrate is placed in the reaction chamber, and then the reaction chamber temperature is heated to 100°C; gaseous titanium tetraisopropoxide is introduced into the reaction chamber for 400 milliseconds, and then purged with Ar at a flow rate of 50 sccm for 30 seconds; gaseous H is introduced into the reaction chamber. 2 O for 100 ms and finally N with a flow rate of 50 sccm 2 Purge for 30 seconds to complete the first deposition of titanium dioxide on the polyphenylsulfone porous membrane substrate;

[0079] Step 3, repeating step 2 to complete 200 depositions to obtain a modified polyphenylene sulfone porous membrane precursor with a titanium dioxide layer deposited on the surface;

[0080] Step 4, spray 3wt% of allyl glycidyl ether onto the surface of the modified polyphenylsulfone porous membrane precursor, irradiate the modified polyphenylsulfone porous membrane precursor with a 500 joule xenon lamp for 30 minutes to perform hydrophilic modification, rinse with anhydrous ethanol, and dry in the shade to obtain a modified polyphenylsulfone porous membrane 3. According to measurement, the porosity of the modified polyphenylsulfone porous membrane 3 is 47.56%, the contact angle is 27.34°, the tensile strength is 7.76MPa, and the elongation at break is 27.48%.

[0081] The cross-sectional SEM image and contact angle image of the modified polyphenylsulfone porous membrane 3 prepared in Example 3 of the present invention are respectively Figure 2 , Figure 3 Similar, no longer given here.

[0082] Example 4

[0083] In this embodiment, a titanium dioxide layer is deposited on the surface of a polyphenylsulfone porous membrane substrate using atomic deposition technology to obtain a modified polyphenylsulfone porous membrane precursor. Then, a modifier is sprayed on the surface of the modified polyphenylsulfone porous membrane precursor by photocatalysis to obtain a modified polyphenylsulfone porous membrane. The surface modifier is 3wt% allyl glycidyl ether. Specifically, as follows:

[0084] Step 1. Weigh polyphenylsulfone, N-methylpyrrolidone and sodium dodecyl sulfate in a mass ratio of 28.5:61.5:10, add them into the reactor in turn and stir, heat to 50-150°C, stir at 200r / min for 4 hours, and then degas to obtain a casting liquid. Then mix N-methylpyrrolidone and water in a volume ratio of 50%, and transfer the mixed solution to the core liquid furnace of the hollow fiber spinning machine as the core liquid. Use the casting liquid as the raw material, use a hollow fiber spinning machine for spinning, extrude the casting liquid, undergo an air process, and immerse it in a water coagulation bath for solidification. Soak the preliminarily solidified membrane filaments in deionized water to remove residual N-methylpyrrolidone and sodium dodecyl sulfate to obtain a polyphenylsulfone porous membrane substrate.

[0085] Step 2: Use an atomic layer deposition apparatus (D100-4882, Chongqing Nuotu Technology Co., Ltd.) as an atomic deposition apparatus. The apparatus is completely sealed relative to the external environment. By controlling the running time of the program in the apparatus, the amount of gaseous titanium-containing precursor and gaseous oxygen-containing precursor introduced can be controlled. The reaction chamber of the atomic deposition apparatus is evacuated to a vacuum degree of 4 mbar, a polyphenylsulfone porous membrane substrate is placed in the reaction chamber, and then the reaction chamber temperature is heated to 100°C; gaseous titanium tetraisopropoxide is introduced into the reaction chamber for 400 milliseconds, and then purged with Ar at a flow rate of 50 sccm for 30 seconds; gaseous H is introduced into the reaction chamber. 2 O for 100 ms and finally N with a flow rate of 50 sccm 2 Purge for 30 seconds to complete the first deposition of the titanium dioxide layer on the polyphenylsulfone porous membrane substrate;

[0086] Step 3, repeating step 2 to complete 200 depositions to obtain a modified polyphenylene sulfone porous membrane precursor with a titanium dioxide layer deposited on the surface;

[0087] Step 4, spraying nano-silicon emulsion onto the surface of the modified polyphenylsulfone porous membrane precursor, irradiating the modified polyphenylsulfone porous membrane precursor with a 500 joule xenon lamp for 30 minutes to hydrophilically modify the modified polyphenylsulfone porous membrane precursor, rinsing with anhydrous ethanol, and drying in the shade to obtain a modified polyphenylsulfone porous membrane 4. According to measurement, the porosity of the modified polyphenylsulfone porous membrane 4 is 40.53%, the contact angle is 28.56°, the tensile strength is 17.83 MPa, and the elongation at break is 32.71%.

[0088] The cross-sectional SEM image and contact angle image of the modified polyphenylsulfone porous membrane 4 prepared in Example 4 of the present invention are respectively Figure 2 , Figure 3 Similar, no longer given here.

[0089] Comparative Example 1

[0090] Prepare the polyphenylsulfone porous membrane substrate as follows:

[0091] Step 1. Weigh polyphenylsulfone, N-methylpyrrolidone and sodium dodecyl sulfate in a mass ratio of 17:73:10, add them into the reactor in turn and stir, heat to 50-150°C, stir at 200r / min for 4 hours, and then degas to obtain a casting liquid. Then mix N-methylpyrrolidone and water in a volume ratio of 50%, and transfer the mixed solution to the core liquid furnace of the hollow fiber spinning machine as the core liquid. Use the casting liquid as the raw material, use a hollow fiber spinning machine for spinning, extrude the casting liquid, undergo an air process, and then immerse it in a water coagulation bath for solidification. Soak the preliminarily solidified membrane filaments in deionized water to remove residual additives and solvents to obtain a polyphenylsulfone porous membrane substrate.

[0092] Figure 4 The cross-sectional SEM image of the polyphenylsulfone porous membrane substrate provided in Comparative Example 1 is shown. As shown in the figure, the cross-sectional SEM image of the modified polyphenylsulfone porous membrane 1 in Example 1 ( Figure 2 ), it can be seen that the structure of the polyphenylsulfone porous membrane substrate has hardly changed, the membrane cross section is a sponge pore structure with good connectivity, the membrane porosity is measured to be 50.33%, the tensile strength is 6.01 MPa, and the elongation at break is 29.29%.

[0093] Figure 5 The contact angle image of the polyphenylsulfone porous membrane substrate provided in Comparative Example 1 is shown. As shown in the figure, the contact angle of the polyphenylsulfone porous membrane substrate is relatively large. After measurement, the contact angle is 72.21°. It can be seen that the hydrophilicity of the polyphenylsulfone porous membrane substrate is relatively poor.

[0094] Comparative Example 2

[0095] This embodiment uses a low-temperature hydrothermal method to directly coat titanium dioxide nanoparticles on the surface of the polyphenylsulfone porous membrane substrate, and then sprays a modifier on the surface of the titanium dioxide nanoparticle layer through photocatalysis. The modifier is a nano-silicon emulsion. Specifically, as follows:

[0096] Step 1. Weigh polyphenylsulfone, N-methylpyrrolidone and sodium dodecyl sulfate in a mass ratio of 17:73:10, add them into the reactor in turn and stir, heat to 50-150°C, stir at 200r / min for 4 hours, and then degas to obtain a casting liquid. Then mix N-methylpyrrolidone and water in a volume ratio of 50%, and transfer the mixed solution to the 20°C core liquid furnace of the hollow fiber spinning machine as the core liquid. Use the casting liquid as the raw material, use a hollow fiber spinning machine for spinning, extrude the casting liquid, undergo an air process, and then immerse it in a water coagulation bath for solidification. Soak the preliminarily solidified membrane filaments in deionized water to remove residual additives and solvents to obtain a polyphenylsulfone porous membrane substrate;

[0097] Step 2: Use low-temperature hydrothermal method to directly coat titanium dioxide nanoparticles on the surface of polyphenylsulfone porous membrane substrate to obtain polyphenylsulfone porous membrane with titanium dioxide nanoparticle layer on the surface; specifically: add 0.1ml ethylenediamine and 1ml isopropyl titanate to 40ml anhydrous ethanol respectively, stir at room temperature for 1h to obtain a solution. Then add the solution to 80ml polytetrafluoroethylene hydrothermal reactor, put in polyphenylsulfone porous membrane substrate, tighten the high-pressure reactor and put in 80℃ oven for 5h, take out and cool at room temperature, rinse the reacted membrane with distilled water and ethanol, dry it, and obtain polyphenylsulfone porous membrane with titanium dioxide nanoparticle layer on the surface.

[0098] Step 3, spraying nano-silicon emulsion onto the surface of the polyphenylsulfone porous membrane coated with a titanium dioxide nanoparticle layer, irradiating the titanium dioxide nanoparticle layer with a 500-joule xenon lamp for 30 minutes to hydrophilically modify the titanium dioxide nanoparticle layer, washing with anhydrous ethanol, and drying in the shade to obtain a modified polyphenylsulfone porous membrane 5. According to measurement, the porosity of the modified polyphenylsulfone porous membrane 5 is 45.25%, the contact angle is 53.28°, the tensile strength is 4.95 MPa, and the elongation at break is 16.34%.

[0099] The cross-sectional SEM image of the modified polyphenylsulfone porous membrane 5 prepared in Comparative Example 2 is Figure 2 Similar to the contact angle graph Figure 5 Similar, no longer given here.

[0100] Test Example 1

[0101] This test example is used to verify the water vapor / air selectivity and water vapor permeability of the samples provided in Examples 1-4 and Comparative Examples 1-2. The verification process is as follows:

[0102] Membrane humidification test: The modified polyphenylsulfone porous membranes 1-4 prepared in Examples 1-4, the polyphenylsulfone porous membrane substrate prepared in Comparative Example 1, and the modified polyphenylsulfone porous membrane 5 prepared in Comparative Example 2 were respectively encapsulated into membrane components with epoxy resin AB glue, and 1 bar of water vapor or air was introduced into the membrane components. The gas flow was monitored with a soap film flowmeter, and the water vapor permeability and water vapor / air selectivity of each composite membrane were calculated to obtain the data in the following table.

[0103] Table 1 Performance parameters of membrane

[0104]

[0105] Combining the data in the above table with the membrane porosity, contact angle, tensile strength and elongation at break data described in the embodiments and comparative examples, it can be seen that the contact angle (53.28°) of the modified polyphenylsulfone porous membrane 5 of comparative example 2 is slightly smaller than that of the unmodified polyphenylsulfone porous membrane substrate (72.21°) in comparative example 1, but its porosity, tensile strength and elongation at break are all worse than those of the unmodified polyphenylsulfone porous membrane substrate.

[0106] The porosity, tensile strength and elongation at break of the modified polyphenylsulfone porous membrane 2 of Example 2 are not much different from those of the unmodified polyphenylsulfone porous membrane substrate, but the hydrophilicity improvement effect is very poor, and the water contact angle (60.59°) of the polyphenylsulfone porous membrane 2 has almost no change. At the same time, there is a common problem between the modified polyphenylsulfone porous membrane 5 and the modified polyphenylsulfone porous membrane 2: the life of the membrane is poor. Although the modified polyphenylsulfone porous membrane 2 uses the atomic deposition technology to deposit a titanium dioxide layer on the surface of the polyphenylsulfone porous membrane substrate, so that the titanium dioxide layer is not easy to fall off during its operation, relative to the modified polyphenylsulfone porous membrane 5, the service life of the membrane can be improved to a certain extent, but after running for 100 hours, the water vapor / air selectivity of the modified polyphenylsulfone porous membrane 2 will decrease, and the water vapor permeability will increase.

[0107] Compared with Example 2 and Comparative Examples 1-2, the modified polyphenylsulfone porous membrane 1 and modified polyphenylsulfone porous membrane 3 prepared in Example 1 and Example 3 respectively have good hydrophilicity, which is reflected in the significant reduction of the water contact angle, which is less than 30°. In addition, there is no obvious decrease in the rigidity and strength of the membrane, which is reflected in the fact that the tensile strength and elongation at break do not change much, and the regular and rigid channel structure can accurately size-screen water vapor and air molecules, giving the membrane high water vapor / air selectivity. In addition, the pore size and porosity of the membrane are basically not changed after modification, and the developed microporous structure of the polyphenylsulfone porous layer in the membrane strengthens the transmembrane transmission of water vapor molecules and also gives the membrane a lower water vapor permeability. Therefore, the modified polyphenylsulfone porous membrane 1 and the modified polyphenylsulfone porous membrane 3 have high water vapor / air selectivity, reaching 1092-1127, and low water vapor permeability, reaching 0.14-0.15. Meanwhile, after running for 100 hours, the water vapor / air selectivity and water vapor permeability of the modified polyphenylene sulfone porous membrane 1 and the modified polyphenylene sulfone porous membrane 3 remain substantially unchanged, and have a long service life.

[0108] The modified polyphenylsulfone porous membrane provided by the present invention combines the atomic deposition technology and the photocatalytic method, and is prepared by optimizing the vacuum degree of the atomic deposition equipment, the type and content of the surface modifier, thereby enhancing the bonding strength between the layers of the membrane, giving the membrane high application stability, and improving the surface hydrophilicity, thereby providing a separation material with excellent water vapor permeability for air humidification.

[0109] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.

[0110] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.

[0111] The modified polyphenylsulfone porous membrane and its preparation method and application provided by the present invention are introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing a modified polysulfone porous membrane, It is characterized in that The modified polysulfone porous membrane is composed of a polysulfone porous membrane substrate and a modified titanium dioxide layer; Wherein, the polysulfone porous membrane substrate is a sponge-like loose structure; The polysulfone material constituting the polysulfone porous membrane substrate is one or more of polyethersulfone, polyphenylsulfone, polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone and sulfonated polysulfone; The preparation method of the modified polysulfone porous membrane comprises: Step 1, placing a polysulfone porous membrane substrate in an atomic deposition equipment reaction chamber at a temperature of 50-200° C. and a vacuum degree of 0-15 mbar, introducing a gaseous titanium-containing precursor into the reaction chamber for 100-1000 milliseconds, introducing an inert gas at a flow rate of 10-300 sccm for purging for 10-200 seconds, introducing a gaseous oxygen-containing precursor for 10-500 milliseconds, and finally introducing the inert gas at a flow rate of 10-300 sccm for a second purge for 10-200 seconds to complete the first deposition of titanium dioxide on the polysulfone porous membrane substrate; Step 2, repeating step 1 to complete 10-500 depositions to obtain a modified polysulfone porous membrane precursor with a titanium dioxide layer deposited on the surface; Step 3, spraying a modifier onto the surface of the modified polysulfone porous membrane precursor, and irradiating the modified polysulfone porous membrane precursor with a 100-1000 joule xenon lamp for 1-300 minutes to hydrophilically modify the modified polysulfone porous membrane precursor, and washing and drying to obtain the modified polysulfone porous membrane; Wherein, the modifier is 0.1-10wt% of allyl glycidyl ether.

2. The method for preparing the modified polysulfone porous membrane according to claim 1, It is characterized in that The polysulfone porous membrane has a porosity of 40-70%, a tensile strength of 5-20 MPa, an elongation at break of 10-70%, and a water contact angle of 10-30°.

3. The method for preparing the modified polysulfone porous membrane according to claim 1, It is characterized in that The titanium-containing precursor is any one of titanium alkoxide, titanium halide and titanium alkylphthalamide.

4. The method for preparing the modified polysulfone porous membrane according to claim 1, It is characterized in that The oxygen-containing precursor is O 3 , H 2 O and H 2 O 2 Any of .

5. The method for preparing the modified polysulfone porous membrane according to claim 1, It is characterized in that The inert gas is Ar and N 2 Any of .

6. The method for preparing the modified polysulfone porous membrane according to claim 1, It is characterized in that The preparation method of the polysulfone porous membrane substrate comprises: The polysulfone material, solvent and additive are uniformly mixed in a mass ratio of 14-35:52-85.9:0.1-34, and stirred for 4 hours at a temperature of 50-150° C. and a stirring speed of 200-300 r / min to obtain a casting solution; the solvent is mixed with water to obtain a core solution; Injecting the core liquid and the casting liquid into a spinneret, extruding the casting liquid through the spinneret, and after an air process, immersing the casting liquid in a water coagulation bath at room temperature for solidification and forming, thereby obtaining the polysulfone porous membrane substrate; The solvent is one or more of dichloromethane, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, carbon tetrachloride, N-methylpyrrolidone, methanol, ethanol and diethylene glycol; The additive is one or more of sodium lauryl sulfate, suberic acid, oxalic acid, polyvinyl pyrrolidone, dibenzylidene sorbitol and benzoic acid.

7. The method for preparing the modified polysulfone porous membrane according to claim 6, It is characterized in that The polysulfone material is one or more of polyethersulfone, polyphenylsulfone, polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone and sulfonated polysulfone.

8. Use of the modified polysulfone porous membrane prepared by the method for preparing the modified polysulfone porous membrane according to claim 1 in a fuel cell membrane humidifier.