High-strength galvanized steel strip and production method thereof

By adjusting the chemical composition of the strip base and the segmented cooling technology during the annealing process, the problems of low strength and poor corrosion resistance of strip steel are solved, which significantly improves the strength and corrosion resistance of galvanized strip steel and extends salt mist resistance. Time reduces safety hazards and engineering costs.

CN117966031BActive Publication Date: 2024-11-01河北海洪新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410328450.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2024-11-01
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

The existing strip steel has low strength and poor corrosion resistance, which poses safety hazards and increased engineering costs.

Method used

By adjusting the chemical composition of the strip matrix, especially the ratio of Ni-V+Yb and the ratio of Co/Eu, and using segmented cooling technology during the annealing process, the bonding force of the galvanized layer and the strength and resistance of the strip steel are improved. Corrosive.

Benefits of technology

It significantly improves the strength and corrosion resistance of galvanized strip steel, extends salt spray resistance time, and reduces safety hazards and engineering costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of metallurgy technology, and proposes a high-strength galvanized steel strip and a production method thereof. The high-strength galvanized steel strip comprises a steel strip matrix and a galvanized layer, and the steel strip matrix comprises the following components in mass percentage: C 0.05% to 0.08%, Si 0.3% to 0.45%, Al 0.15% to 0.25%, Mn 0.95% to 1.20%, Nb 0.03% to 0.035%, B 0.001% to 0.002%, Mo 0.05% to 0.1%, Cr 0.15% to 0.35%, Yb 0.005% to 0.015%, Ti 0.02% to 0.30%, Ni 1.5% to 2.5%, V 0.05% to 0.1%, Co 0.01% to 0.5%, and Eu 0.01% to 0.018%. Through the above technical scheme, the problems of low strength and poor corrosion resistance of steel strip in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a high-strength galvanized steel strip and a production method thereof. Background Art

[0002] Steel is widely used in many fields such as construction and transportation. Although strip steel has certain strength and corrosion resistance, it still has problems of low strength and poor corrosion resistance, which will cause safety hazards in the application projects, and increase the project cost and construction period invisibly.

[0003] Therefore, with the development of industries such as construction and the improvement of people's safety awareness, higher requirements are put forward for the strength and corrosion resistance of strip steel. At present, in order to improve the strength and corrosion resistance of strip steel, one is to improve the strength of the strip steel matrix; the other is to add high-quality metal coating on the surface of the strip steel matrix to adapt to the rapid development of the industry, reduce safety hazards and expand the application field of strip steel. Summary of the invention

[0004] The invention provides a high-strength galvanized steel strip and a production method thereof, which solves the problems of low strength and poor corrosion resistance of the steel strip in the related art.

[0005] The technical solution of the present invention is as follows:

[0006] The invention provides a high-strength galvanized steel strip, comprising a steel strip matrix and a galvanized layer, wherein the steel strip matrix is ​​composed of the following components in mass percentage: C 0.05%-0.08%, Si 0.3%-0.45%, Al 0.15%-0.25%, Ca 0.01%-0.015%, Mn 0.95%-1.20%, Nb 0.03%-0.035%, B 0.001%-0.002%, Mo 0.05%-0.1%, Cr 0.15%-0.35%, Yb 0.005%-0.015%, Ti 0.02%-0.30%, Ni 1.5%-2.5%, V 0.05%-0.1%, Co 0.01%-0.5%, Eu 0.01%~0.018%, the balance is Fe and other inevitable impurities; and must also meet the following requirements: 1.455%≤Ni-V+Yb≤2.415%, 1≤Co / Eu≤27.78.

[0007] As a further technical solution, the strip steel matrix is ​​composed of the following components in mass percentage: C 0.05%~0.08%, Si 0.3%~0.45%, Al 0.15%~0.25%, Ca 0.01%~0.015%, Mn 0.95%~1.20%, Nb 0.03%~0.035%, B 0.001%~0.002%, Mo 0.05%~0.1%, Cr 0.15%~0.35%, Yb 0.008%~0.012%, Ti 0.15%~0.016%, Ni 1.7%~2%, V 0.07%~0.08%, Co 0.2%~0.35%, Eu 0.012%~0.018%, the balance is Fe and other inevitable impurities; and must also meet the following requirements: 1.7%≤Ni-V+Yb≤1.942%, 16.67≤Co / Eu≤19.44.

[0008] In the present invention, the strength of the galvanized steel strip is further improved by making 1.7%≤Ni-V+Yb≤1.942% and 16.67≤Co / Eu≤19.44 in the steel strip matrix.

[0009] The present invention also provides a method for producing the high-strength galvanized steel strip, comprising the following steps:

[0010] S1. Smelting, casting, hot rolling and cold rolling are performed according to the components of the strip steel matrix to obtain the strip steel matrix;

[0011] S2. After annealing, the steel strip substrate is immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip.

[0012] As a further technical solution, the temperature of the zinc liquid is 460-480°C.

[0013] As a further technical solution, during the annealing, the steel strip substrate is subjected to soaking, first cooling, second cooling and heating to the zinc liquid temperature in sequence;

[0014] The temperature during the soaking is 700-750°C and the time is 70-80s;

[0015] The first cooling is performed to cool to 550-600° C.

[0016] The second cooling is performed to cool to 400-420°C.

[0017] As a further technical solution, the cooling rate of the first cooling is greater than the cooling rate of the second cooling.

[0018] As a further technical solution, the cooling rate of the first cooling is 20-30°C / s.

[0019] As a further technical solution, the cooling rate of the second cooling is 12-14°C / s.

[0020] As a further technical solution, the cooling rate of the second cooling is 8-10°C / s.

[0021] As a further technical solution, the cooling rate of the second cooling is 9°C / s.

[0022] In the present invention, by adopting segmented cooling during annealing, the quality of the strip steel substrate and the galvanized layer is improved, and the strength and corrosion resistance of the galvanized strip steel are further improved.

[0023] As a further technical solution, the zinc liquid is composed of the following components in mass percentage: Al 0.01%-0.013%, Sb 0.03%-0.06%, and the balance is Zn and other inevitable impurities.

[0024] The working principle and beneficial effects of the present invention are:

[0025] 1. In the present invention, by making 1.455%≤Ni-V+Yb≤2.415% and 1≤Co / Eu≤27.78 in the strip steel matrix, the strip steel matrix is ​​strengthened and the bonding strength with the galvanized layer is improved, thereby significantly improving the strength and corrosion resistance of the galvanized strip steel. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] High-strength galvanized steel strip, comprising a steel strip matrix and a galvanized layer, wherein the steel strip matrix is ​​composed of the following components in mass percentage: C 0.05%, Si 0.3%, Al 0.15%, Ca 0.01%, Mn 0.95%, Nb 0.03%, B 0.001%, Mo 0.05%, Cr0.15%, Yb 0.005%, Ti 0.02%, Ni 1.5%, V 0.05%, Co 0.01%, Eu 0.01%, the balance being Fe and other unavoidable impurities; and the following conditions must be met at the same time: Ni-V+Yb=1.455%, Co / Eu=1;

[0029] The production method of high-strength galvanized steel strip comprises the following steps:

[0030] S1. Smelting, casting, hot rolling and cold rolling are performed according to the components of the strip steel matrix to obtain the strip steel matrix;

[0031] S2. After the steel strip substrate is heated at 700°C for 80 seconds, it is first cooled to 550°C at a cooling rate of 5°C / s, and kept warm for 20 seconds. Then, it is cooled to 400°C at a cooling rate of 5°C / s, and kept warm for 10 seconds. Then, the steel strip substrate is heated to a zinc liquid temperature of 460°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.01%, Sb 0.03%, and the balance is Zn and other inevitable impurities.

[0032] Example 2

[0033] High-strength galvanized steel strip, comprising a steel strip matrix and a galvanized layer, wherein the steel strip matrix is ​​composed of the following components in mass percentage: C 0.06%, Si 0.4%, Al 0.2%, Ca 0.013%, Mn 1%, Nb 0.033%, B 0.001%, Mo 0.07%, Cr0.25%, Yb 0.01%, Ti 0.15%, Ni 2.0%, V 0.06%, Co 0.0156%, Eu 0.015%, the balance being Fe and other unavoidable impurities; and the following conditions must be met at the same time: Ni-V+Yb=1.95%, Co / Eu=1.04;

[0034] The production method of high-strength galvanized steel strip comprises the following steps:

[0035] S1. Smelting, casting, hot rolling and cold rolling are performed according to the components of the strip steel matrix to obtain the strip steel matrix;

[0036] S2. After the steel strip substrate is heated at 750°C for 70s, it is first cooled to 600°C at a cooling rate of 5°C / s, and kept warm for 20s. Then, it is cooled to 420°C at a cooling rate of 5°C / s, and kept warm for 10s. Then, the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0037] Example 3

[0038] High-strength galvanized steel strip, comprising a steel strip matrix and a galvanized layer, wherein the steel strip matrix is ​​composed of the following components in mass percentage: C 0.08%, Si 0.45%, Al 0.25%, Ca 0.015%, Mn 1.20%, Nb 0.035%, B 0.002%, Mo 0.1%, Cr0.35%, Yb 0.015%, Ti 0.30%, Ni 2.5%, V 0.1%, Co 0.5%, Eu 0.018%, the balance being Fe and other unavoidable impurities; and the following conditions must be met at the same time: Ni-V+Yb=2.415%, Co / Eu=27.78;

[0039] The production method of high-strength galvanized steel strip comprises the following steps:

[0040] S1. Smelting, casting, hot rolling and cold rolling are performed according to the components of the strip steel matrix to obtain the strip steel matrix;

[0041] S2. After the steel strip substrate is heated at 750°C for 70s, it is first cooled to 600°C at a cooling rate of 5°C / s, and kept warm for 20s. Then, it is cooled to 420°C at a cooling rate of 5°C / s, and kept warm for 10s. Then, the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0042] Example 4

[0043] The only difference between this embodiment and embodiment 3 is that the strip steel matrix is ​​composed of the following components in mass percentage: C 0.08%, Si 0.45%, Al 0.25%, Ca 0.015%, Mn 1.20%, Nb 0.035%, B 0.002%, Mo 0.1%, Cr 0.35%, Yb 0.015%, Ti 0.30%, Ni 1.55%, V 0.065%, Co 0.17%, Eu 0.013%, and the balance is Fe and other inevitable impurities; and the following conditions must be satisfied at the same time: Ni-V+Yb=1.5%, Co / Eu=13.08.

[0044] Example 5

[0045] The only difference between this embodiment and embodiment 3 is that the strip steel matrix is ​​composed of the following components in mass percentage: C 0.08%, Si 0.45%, Al 0.25%, Ca 0.015%, Mn 1.20%, Nb 0.035%, B 0.002%, Mo 0.1%, Cr 0.35%, Yb 0.008%, Ti 0.15%, Ni 1.7%, V 0.08%, Co 0.2%, Eu 0.012%, and the balance is Fe and other inevitable impurities; and the following conditions must be satisfied at the same time: Ni-V+Yb=1.628%, Co / Eu=16.67.

[0046] Example 6

[0047] The only difference between this embodiment and embodiment 3 is that the strip steel matrix is ​​composed of the following components in mass percentage: C 0.08%, Si 0.45%, Al 0.25%, Ca 0.015%, Mn 1.20%, Nb 0.035%, B 0.002%, Mo 0.1%, Cr0.35%, Yb 0.012%, Ti 0.15%, Ni 2%, V 0.07%, Co 0.35%, Eu 0.018%, and the balance is Fe and other inevitable impurities; and the following conditions must be satisfied at the same time: Ni-V+Yb=1.942%, Co / Eu=19.44.

[0048] Example 7

[0049] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 5°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 15°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0050] Example 8

[0051] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 15°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 5°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0052] Example 9

[0053] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 20°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 5°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0054] Example 10

[0055] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 30°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 5°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0056] Embodiment 11

[0057] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 30°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 8°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0058] Example 12

[0059] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 20°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 10°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0060] Embodiment 13

[0061] The difference between this embodiment and embodiment 6 is that step S2 of the production method of high-strength galvanized steel strip is: after the steel strip substrate is heated at 750°C for 70s, the steel strip substrate is first cooled to 600°C at a cooling rate of 20°C / s, and kept warm for 20s, and then cooled to 420°C at a cooling rate of 9°C / s, and kept warm for 10s, and then the steel strip substrate is heated to a zinc liquid temperature of 480°C, immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip; wherein the zinc liquid is composed of the following components in mass percentage: Al 0.013%, Sb 0.06%, and the balance is Zn and other inevitable impurities.

[0062] Comparative Example 1

[0063] The difference between this comparative example and Example 3 is that the strip steel matrix is ​​composed of the following components in mass percentage: C 0.08%, Si 0.45%, Al 0.25%, Ca 0.015%, Mn 1.20%, Nb 0.035%, B 0.002%, Mo 0.1%, Cr 0.35%, Yb 0.015%, Ni 2.5%, V 0.1%, and the balance is Fe and other inevitable impurities; and it must also meet the following conditions: Ni-V+Yb=2.415%.

[0064] Comparative Example 2

[0065] The difference between this comparative example and Example 3 is that the strip steel matrix is ​​composed of the following components in mass percentage: C 0.08%, Si 0.45%, Al 0.25%, Ca 0.015%, Mn 1.20%, Nb 0.035%, B 0.002%, Mo 0.1%, Cr 0.35%, Ti 0.30%, Co 0.5%, Eu 0.018%, and the balance is Fe and other inevitable impurities; and it must also satisfy: Co / Eu=27.78.

[0066] The performance tests were performed on the galvanized steel strips prepared in Examples 1 to 13 and Comparative Examples 1 to 2, respectively, and the test methods were as follows:

[0067] The tensile strength test (longitudinal direction) is carried out in accordance with the standard GB / T 228.1-2021 "Tensile tests on metallic materials - Part 1: Test methods at room temperature";

[0068] Salt spray resistance test: The YWST-86 salt spray test device was used for the experiment. The experimental process was set as follows: spray for 15 minutes every 15 minutes. The spray medium was a 10wt% NaCl solution. The corrosion of the sample surface was observed and the time when the corrosion began to appear on the sample surface was recorded.

[0069] The test results are shown in the following table:

[0070]

[0071] By comparing the data of Examples 1 to 13 and Comparative Examples 1 to 2, it can be seen that compared with Comparative Examples 1 to 2, the galvanized steel strips prepared in Examples 1 to 13 have higher tensile strength and longer salt spray resistance time, indicating that by adding 1.455% to 2.415% by mass of Ni-V+Yb to the steel strip matrix and when 1≤Co / Eu≤27.78, the strength and corrosion resistance of the galvanized steel strip can be significantly improved.

[0072] By comparing the data of Examples 3 to 6, it can be seen that compared with Examples 3 to 4, the galvanized steel strips prepared in Examples 5 to 6 have higher tensile strength and longer salt spray resistance time, indicating that the strength of the galvanized steel strips can be further improved by further adjusting the mass percentage of Ni-V+Yb in the steel strip matrix to 1.7% to 1.942% and the Co / Eu ratio to 16.67 to 19.44.

[0073] By comparing the data of Examples 6 to 13, it can be seen that compared with Examples 6 to 7, the galvanized steel strips prepared in Examples 8 to 13 have higher tensile strength and longer salt spray resistance time, indicating that by making the cooling rate of the first cooling greater than the cooling rate of the second cooling during annealing, the strength and corrosion resistance of the galvanized steel strip can be further improved; compared with Examples 9 to 10, the galvanized steel strips prepared in Examples 11 to 13 have higher tensile strength and longer salt spray resistance time, indicating that by making the cooling rate of the first cooling to 20 to 30°C / s and the cooling rate of the second cooling to 8 to 10°C / s during annealing, the strength and corrosion resistance of the galvanized steel strip can be further improved.

[0074] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength galvanized steel strip, characterized in that: The invention comprises a strip steel matrix and a galvanized layer, wherein the strip steel matrix is ​​composed of the following components in mass percentage: C 0.05%-0.08%, Si 0.3%-0.45%, Al 0.15%-0.25%, Ca 0.01%-0.015%, Mn 0.95%-1.20%, Nb 0.03%-0.035%, B 0.001%-0.002%, Mo 0.05%-0.1%, Cr 0.15%-0.35%, Yb 0.005%-0.015%, Ti 0.02%-0.30%, Ni 1.5%-2.5%, V 0.05%-0.1%, Co 0.01%-0.5%, Eu 0.01%~0.018%, the balance is Fe and other inevitable impurities; and must also meet the following requirements: 1.455%≤Ni-V+Yb≤2.415%, 1≤Co / Eu≤27.78; The production method of the high-strength galvanized steel strip comprises the following steps: S1. Smelting, casting, hot rolling and cold rolling are performed according to the components of the strip steel matrix to obtain the strip steel matrix; S2, annealing the steel strip substrate, immersing it in zinc liquid, taking it out and cooling it to obtain a galvanized steel strip; During the annealing, the steel strip substrate is subjected to soaking, first cooling, second cooling and heating to the temperature of the zinc liquid in sequence; The temperature during the soaking is 700-750°C and the time is 70-80s; The first cooling is performed to cool to 550-600° C. The second cooling is performed to cool to 400-420°C; The cooling rate of the first cooling is greater than the cooling rate of the second cooling.

2. The high-strength galvanized steel strip according to claim 1, characterized in that: The strip steel matrix is ​​composed of the following components in mass percentage: C 0.05%~0.08%, Si 0.3%~0.45%, Al 0.15%~0.25%, Ca 0.01%~0.015%, Mn 0.95%~1.20%, Nb 0.03%~0.035%, B 0.001%~0.002%, Mo 0.05%~0.1%, Cr 0.15%~0.35%, Yb 0.008%~0.012%, Ti 0.15%~0.30%, Ni 1.7%~2%, V 0.07%~0.08%, Co 0.2%~0.35%, Eu 0.012%~0.018%, the balance is Fe and other inevitable impurities; and must also meet the following requirements: 1.7%≤Ni-V+Yb≤1.942%, 16.67≤Co / Eu≤19.

44.

3. The method for producing high-strength galvanized steel strip according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Smelting, casting, hot rolling and cold rolling are performed according to the components of the strip steel matrix to obtain the strip steel matrix; S2. After annealing, the steel strip substrate is immersed in zinc liquid, taken out and cooled to obtain a galvanized steel strip.

4. The method for producing high-strength galvanized steel strip according to claim 3, characterized in that: The temperature of the zinc solution is 460-480°C.

5. The method for producing high-strength galvanized steel strip according to claim 3, characterized in that: During the annealing, the steel strip substrate is subjected to soaking, first cooling, second cooling and heating to the temperature of the zinc liquid in sequence; The temperature during the soaking is 700-750°C and the time is 70-80s; The first cooling is performed to cool to 550-600° C. The second cooling is performed to cool to 400-420°C.

6. The method for producing high-strength galvanized steel strip according to claim 5, characterized in that: The cooling rate of the first cooling is greater than the cooling rate of the second cooling.

7. The method for producing high-strength galvanized steel strip according to claim 6, characterized in that: The cooling rate of the first cooling is 20-30°C / s.

8. The method for producing high-strength galvanized steel strip according to claim 7, characterized in that: The cooling rate of the second cooling is 12-14°C / s.

9. The method for producing high-strength galvanized steel strip according to claim 6, characterized in that: The cooling rate of the second cooling is 8-10°C / s.

10. The method for producing high-strength galvanized steel strip according to claim 3, characterized in that: The zinc liquid is composed of the following components in mass percentage: Al 0.01%-0.013%, Sb 0.03%-0.06%, and the balance is Zn.