A temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and its preparation method

By introducing a temperature-driven mechanism into the absorbing material, and utilizing the phase change behavior of vanadium dioxide and the composite of carbon nanotubes and aramid nanofibers, a smart aerogel that can regulate the absorbing performance under temperature changes is prepared to solve the problem. The problem that existing absorbing materials cannot be dynamically controlled has achieved the effects of frequency adjustment and function switching.

CN117986678BActive Publication Date: 2024-10-11NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410172551.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-07
Publication Date
2024-10-11
Estimated Expiration
2044-02-07

AI Technical Summary

Technical Problem

The absorbing properties of existing absorbing materials are fixed after preparation and cannot be dynamically adjusted, making it difficult to meet the needs of complex application environments, especially in electromagnetic wave pollution and radiation treatment.

Method used

Using a temperature-driven intelligent tunable electromagnetic wave absorbing composite aerogel, the vanadium dioxide powder is surface-modified and compounded with carboxylated carbon nanotubes and aramid nanofibers, and a porous structure is prepared through hydrothermal method and freeze-drying. The aerogel uses the phase change behavior of vanadium dioxide to regulate the dielectric properties at different temperatures to achieve adjustable absorption frequency and functional switching.

Benefits of technology

It achieves intelligent real-time control of electromagnetic wave absorption performance, enables frequency tunability and functional switching under temperature changes, and improves the dynamic control capability of electromagnetic wave absorption materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117986678B_ABST
    Figure CN117986678B_ABST
Patent Text Reader

Abstract

The present invention discloses a temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and a preparation method thereof, comprising: surface modification of vanadium dioxide powder to obtain vanadium dioxide with amino functional groups on the surface; compounding vanadium dioxide with amino functional groups on the surface with carboxylated carbon nanotubes to obtain an absorbing filler; and freeze-drying the absorbing filler and aramid nanofiber dispersion to obtain a CNTs / VO2 / ANF mixed aerogel. The aerogel prepared by the present invention has different dielectric properties at different temperatures, which opens a way for the intelligent control application of electromagnetic absorbers driven by temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electromagnetic wave absorbing materials, and specifically relates to a temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and a preparation method thereof. Background Art

[0002] The rapid development of the information age has led to the widespread application of electromagnetic wave technology in communication technology, electronic equipment, military and other fields. However, the intensified electromagnetic wave pollution and radiation also pose a threat to human health and information security. The urgent need to efficiently deal with electromagnetic pollution and absorb electromagnetic wave radiation has attracted great attention to the development of efficient electromagnetic wave absorbing materials. At present, the absorbing properties of most absorbing materials are fixed after preparation and cannot be dynamically adjusted. Faced with complex practical application environments and fields, a single electromagnetic wave absorption performance can no longer meet the requirements. Therefore, new requirements for intelligent controllability are put forward for current electromagnetic wave absorbing materials.

[0003] Aerogel has the physical properties of ultra-low density, high porosity, large specific surface area and low dielectric constant, and has great potential for regulating electromagnetic wave absorption. 2 ) is a phase change material that undergoes a temperature-driven metal-insulator phase transition (MIT) at around 68°C. At the same time, its conductivity changes dramatically during the phase change, making VO 2 It has potential uses in the field of wave absorption. Therefore, the present invention proposes a temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and a preparation method thereof to achieve intelligent real-time adjustable function of electromagnetic absorption. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and a preparation method thereof, which solves the problem that it is difficult to implement adjustable absorbing performance of traditional absorbing materials. The aerogel prepared by this method can realize two functions based on temperature drive: adjustable absorbing frequency and switchable absorbing function.

[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0006] (I) A temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and a preparation method thereof, comprising: surface-modifying vanadium dioxide powder to obtain vanadium dioxide with amino functional groups on the surface; compounding the vanadium dioxide with amino functional groups on the surface with carboxylated carbon nanotubes to obtain an absorbing filler; uniformly mixing the absorbing filler with an aramid nanofiber dispersion and freeze-drying the mixture to obtain CNTs / VO 2 / ANF hybrid aerogel.

[0007] Furthermore, the preparation method of the vanadium dioxide powder is as follows: adding vanadium pentoxide and citric acid monohydrate to deionized water, magnetically stirring until orange-yellow, then performing a hydrothermal reaction, centrifugally drying, performing a high-temperature annealing treatment, and grinding the treated solid to obtain VO 2 powder.

[0008] Furthermore, the mass ratio of citric acid monohydrate to vanadium pentoxide is 1.775:1; the hydrothermal reaction temperature is 180°C; the high temperature annealing treatment procedure is 450°C for 3 to 5 hours, and the heating rate is not higher than 3°C / min; the protective gas for high temperature annealing is argon or nitrogen.

[0009] Furthermore, the method for surface modification of vanadium dioxide powder is: mixing vanadium dioxide with anhydrous ethanol and ultrasonicating, then adding APTES, magnetically stirring and centrifuging to obtain vanadium dioxide with amino functional groups on the surface.

[0010] Furthermore, the ratio of vanadium dioxide powder to APTES was 0.473 g:25 μL.

[0011] Furthermore, the composite method of vanadium dioxide with amino functional groups on the surface and carboxylated carbon nanotubes is: mixing vanadium dioxide with amino functional groups on the surface and carboxylated carbon nanotubes in water, stirring magnetically in a water bath, and then washing and drying to obtain a wave absorbing filler.

[0012] Furthermore, the water bath temperature is 90° C., and the magnetic stirring time is 1 h.

[0013] Furthermore, the preparation method of the aramid nanofiber dispersion is: adding aramid fibers to a dimethyl sulfoxide solution containing potassium hydroxide, stirring to crack the aramid fibers into aramid nanofibers, and washing with deionized water to replace the dimethyl sulfoxide solution to obtain the aramid nanofiber dispersion.

[0014] Furthermore, in the dimethyl sulfoxide solution containing potassium hydroxide, the mass concentration of potassium hydroxide is 2-3 mg / ml; and the stirring time is 5-7 days.

[0015] Furthermore, the freeze-drying temperature is -50 to -30°C.

[0016] Furthermore, the ratio of the carboxylated carbon nanotubes, vanadium dioxide with amino functional groups on the surface and aramid nanofiber dispersion is (0.024-0.040) g: (0.072-0.120) g: 16 g; in the aramid nanofiber dispersion, the mass concentration of aramid nanofiber is 9-11 mg / g.

[0017] Furthermore, the ratio of the carboxylated carbon nanotubes, vanadium dioxide with amino functional groups on the surface and aramid nanofiber dispersion is (0.024-0.040) g: (0.120-0.200) g: 16 g; in the aramid nanofiber dispersion, the mass concentration of aramid nanofiber is 9-11 mg / g.

[0018] Furthermore, the ratio of the carboxylated carbon nanotubes, vanadium dioxide with amino functional groups on the surface and aramid nanofiber dispersion is (0.072-0.088) g: (0.360-0.440) g: 16 g; in the aramid nanofiber dispersion, the mass concentration of aramid nanofiber is 9-11 mg / g.

[0019] (ii) The present invention also provides an aerogel with adjustable wave absorption frequency, which is prepared by the above method.

[0020] (III) The present invention also provides an aerogel whose wave absorbing function can be switched from closed to open, which is prepared by the above method.

[0021] (III) The present invention also provides an aerogel with a wave absorbing function that can be switched from on to off, which is prepared by the above method.

[0022] Beneficial effects:

[0023] The present invention prepares an aerogel structure with a porous structure and adjustable wave-absorbing performance through a hydrothermal method and a freeze-drying method, wherein vanadium dioxide is used as a regulating filler, and carboxylated carbon nanotubes are used as wave-absorbing fillers and are evenly distributed on aramid nanofibers as aerogel skeletons with vanadium dioxide. Thanks to the phase change behavior of vanadium dioxide, it has different dielectric properties at different temperatures, which is conducive to the application of intelligent regulation of wave-absorbing performance. The aerogel with an aramid nanofiber skeleton has a porous structure, which helps electromagnetic waves enter the interior of the material. By adding wave-absorbing fillers, different VO 2 The filling amount of aerogel induces different degrees of multipolarization effects, enabling frequency tunability of electromagnetic wave absorption performance and switchable switching function under temperature drive. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a preparation flow chart of the method of the present invention;

[0025] Figures 2-3 is a photo of the aerogel prepared in Example 1;

[0026] Figure 4 This is a photo of the aerogel prepared in Comparative Example 1;

[0027] Figure 5 The SEM and EDS images of the wave absorbing filler prepared in Example 2 are shown;

[0028] Figure 6 is the electromagnetic parameter diagram of Example 1;

[0029] Figure 7 is the electromagnetic parameter diagram of Example 2;

[0030] Figure 8 is the electromagnetic parameter diagram of Example 3;

[0031] Fig. 9 It is the electromagnetic parameter diagram of comparative example 1;

[0032] Fig.10 It is a graph of the wave absorption performance of Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] The experimental methods used in the following examples are conventional methods unless otherwise specified, and the reagents, methods and equipment used are conventional reagents, methods and equipment in the art unless otherwise specified.

[0035] Example 1

[0036] This embodiment provides an aerogel with frequency tunable function, and the preparation method includes:

[0037] (1) Preparation of vanadium dioxide powder:

[0038] In a 100ml beaker, 56ml of deionized water, 1.065g of monohydrated citric acid and 0.6g of vanadium pentoxide were added successively. After magnetic stirring for 15min, the solution changed from turbid to orange-yellow. The solution was then transferred to a 100ml polytetrafluoroethylene reactor, which was sealed and placed in a forced air drying oven at 180°C for 6h. After the reaction was completed, it was naturally cooled to room temperature, the dark blue transparent supernatant was poured off, and the black product at the bottom was washed alternately with deionized water and anhydrous ethanol three times. After drying at 60°C in a vacuum drying oven for 6h, it was ground using an agate mortar to obtain phase B VO 2 Powder (VO 2 (B)). Then, 2 The M phase VO was obtained by annealing at 450℃ for 5h in atmosphere and grinding. 2 Powder (VO 2 (M)).

[0039] (2) Surface modification of vanadium dioxide:

[0040] Add 0.473 g of VO2 into a 250 ml beaker. 2 (M), 100 ml of anhydrous ethanol and 1 ml of deionized water, ultrasonically disperse for 1 hour. Then add 25 μL of APTES, magnetically stir for 5 hours, centrifuge; wash with anhydrous ethanol three times, dry in a vacuum oven at 40°C for 8 hours, and grind to obtain VO 2 @APTES powder (VA).

[0041] (3) Preparation of absorbing materials:

[0042] Carboxylated carbon nanotubes (COOH-CNTS) and VA were added to a beaker containing an appropriate amount of deionized water in a mass ratio of 1:3, magnetically stirred in a water bath at 90°C for 1 hour, and then dried in a vacuum drying oven at 80°C for 4 hours. After grinding, carboxylated carbon nanotubes and vanadium dioxide modified powders in a mass ratio of 1:3 were obtained.

[0043] (4) Preparation of aramid nanofiber solution:

[0044] In a three-necked flask, 1.5 L of dimethyl sulfoxide solution, 3 g of aramid nanofibers, and 4.5 g of potassium hydroxide were respectively added, and mechanical stirring was performed with a stirring paddle for 5 days to crack the aramid fibers. Afterwards, deionized water was used to repeatedly wash the mixture in a suction flask to replace the dimethyl sulfoxide in the mixed solution, and an appropriate amount of deionized water was added to adjust the concentration of the obtained aramid nanofiber (ANF) solution to 10 mg / g.

[0045] (5) Preparation of CNTs / VO 2 / ANF hybrid aerogel:

[0046] 16g of ANF solution was placed in a homemade 4*4*2cm mold, and 0.128g of the absorbent material prepared in step (3) (modified powder with a mass ratio of carboxylated carbon nanotubes to vanadium dioxide of 1:3) was added. After stirring evenly, the sample was frozen at -40°C and then freeze-dried for 120h to obtain CNTs / VO with frequency tunable function. 2 / ANF aerogel. Figures 2-3 ,Depend on Figure 3 It can be seen that the CNTs / VO prepared in this example 2 / ANF aerogel is lightweight.

[0047] Example 2

[0048] This embodiment provides an aerogel with a wave absorbing function that can be turned from off to on, and the preparation method includes:

[0049] (1) Preparation of vanadium dioxide powder:

[0050] In a 100ml beaker, 56ml of deionized water, 1.065g of monohydrated citric acid and 0.6g of vanadium pentoxide were added successively. After magnetic stirring for 15min, the solution changed from turbid to orange-yellow. The solution was then transferred to a 100ml polytetrafluoroethylene reactor, which was sealed and placed in a forced air drying oven at 180°C for 6h. After the reaction was completed, it was naturally cooled to room temperature, the dark blue transparent supernatant was poured off, and the black product at the bottom was washed alternately with deionized water and anhydrous ethanol three times. After drying at 60°C in a vacuum drying oven for 6h, it was ground using an agate mortar to obtain phase B VO 2 Powder (VO 2 (B)). Then, 2 The M phase VO was obtained by annealing at 450℃ for 5h in atmosphere and grinding. 2 Powder (VO 2 (M)).

[0051] (2) Surface modification of vanadium dioxide:

[0052] Add 0.473 g of VO2 into a 250 ml beaker. 2 (M), 100 ml of anhydrous ethanol and 1 ml of deionized water, ultrasonically disperse for 1 hour. Then add 25 μL of APTES, magnetically stir for 5 hours, centrifuge; wash with anhydrous ethanol three times, dry in a vacuum oven at 40°C for 8 hours, and grind to obtain VO 2 @APTES powder (VA).

[0053] (3) Preparation of absorbing materials:

[0054] Carboxylated carbon nanotubes (COOH-CNTS) and VA were added to a beaker containing an appropriate amount of deionized water at a mass ratio of 1:5, and magnetically stirred for 1 h in a water bath at 90 °C, followed by drying in a vacuum oven at 80 °C for 4 h. After grinding, a carboxylated carbon nanotube and vanadium dioxide modified powder ( Figure 5 ).

[0055] (4) Preparation of aramid nanofiber solution:

[0056] In a three-necked flask, 1.5 L of dimethyl sulfoxide solution, 3 g of aramid nanofibers, and 4.5 g of potassium hydroxide were respectively added, and mechanical stirring was performed with a stirring paddle for 5 days to crack the aramid fibers. Afterwards, deionized water was used to repeatedly wash the mixture in a suction flask to replace the dimethyl sulfoxide in the mixed solution, and an appropriate amount of deionized water was added to adjust the concentration of the obtained aramid nanofiber solution to 10 mg / g.

[0057] (5) Preparation of CNTs / VO 2 / ANF hybrid aerogel:

[0058] 16g of ANF solution was placed in a homemade 4*4*2cm mold, and 0.192g of the absorbent material prepared in step (3) (modified powder with a mass ratio of carboxylated carbon nanotubes to vanadium dioxide of 1:5) was added. After stirring evenly, the sample was frozen at -40°C and then freeze-dried for 120h to obtain CNTs / VO2 with the absorbent function turned from off to on. 2 / ANF aerogel.

[0059] Example 3

[0060] This embodiment provides an aerogel with a wave absorbing function that can be turned on and off, and the preparation method includes:

[0061] (1) Preparation of vanadium dioxide powder:

[0062] In a 100ml beaker, 56ml of deionized water, 1.065g of monohydrated citric acid and 0.6g of vanadium pentoxide were added successively. After magnetic stirring for 15min, the solution changed from turbid to orange-yellow. The solution was then transferred to a 100ml polytetrafluoroethylene reactor, which was sealed and placed in a forced air drying oven at 180°C for 6h. After the reaction was completed, it was naturally cooled to room temperature, the dark blue transparent supernatant was poured off, and the black product at the bottom was washed alternately with deionized water and anhydrous ethanol three times. After drying at 60°C in a vacuum drying oven for 6h, it was ground using an agate mortar to obtain phase B VO 2 Powder (VO 2 (B)). Then, 2 The M phase VO was obtained by annealing at 450℃ for 5h in atmosphere and grinding. 2 Powder (VO 2 (M)).

[0063] (2) Surface modification of vanadium dioxide:

[0064] Add 0.473 g of VO2 into a 250 ml beaker. 2 (M), 100 ml of anhydrous ethanol and 1 ml of deionized water, ultrasonically disperse for 1 hour. Then add 25 μL of APTES, magnetically stir for 5 hours, centrifuge; wash with anhydrous ethanol three times, dry in a vacuum oven at 40°C for 8 hours, and grind to obtain VO 2 @APTES powder (VA).

[0065] (3) Preparation of absorbing materials:

[0066] Carboxylated carbon nanotubes (COOH-CNTS) and VA were added to a beaker containing an appropriate amount of deionized water in a mass ratio of 1:5, magnetically stirred in a water bath at 90°C for 1 hour, and then dried in a vacuum drying oven at 80°C for 4 hours. After grinding, carboxylated carbon nanotubes and vanadium dioxide modified powders in a mass ratio of 1:5 were obtained.

[0067] (4) Preparation of aramid nanofiber solution:

[0068] In a three-necked flask, 1.5 L of dimethyl sulfoxide solution, 3 g of aramid nanofibers, and 4.5 g of potassium hydroxide were respectively added, and mechanical stirring was performed with a stirring paddle for 5 days to crack the aramid fibers. Afterwards, deionized water was used to repeatedly wash the mixture in a suction flask to replace the dimethyl sulfoxide in the mixed solution, and an appropriate amount of deionized water was added to adjust the concentration of the obtained aramid nanofiber solution to 10 mg / g.

[0069] (5) Preparation of CNTs / VO 2 / ANF hybrid aerogel:

[0070] 16g of ANF solution was placed in a homemade 4*4*2cm mold, and 0.48g of the absorbent material prepared in step (3) (modified powder with a mass ratio of carboxylated carbon nanotubes to vanadium dioxide of 1:5) was added. After stirring evenly, the sample was frozen at -40°C and then freeze-dried for 120h to obtain CNTs / VO2 with the absorbent function turned on and off. 2 / ANF aerogel.

[0071] Comparative Example 1

[0072] This comparative example provides a preparation method of carbon nanotube / aramid nanofiber aerogel, comprising the following steps:

[0073] (1) Preparation of aramid nanofiber dispersion:

[0074] In a three-necked flask, 1.5 L of dimethyl sulfoxide solution, 3 g of aramid nanofibers, and 4.5 g of potassium hydroxide were respectively added, and mechanical stirring was performed with a stirring paddle for 5 days to crack the aramid fibers. Afterwards, deionized water was used to repeatedly wash the mixture in a suction flask to replace the dimethyl sulfoxide in the mixed solution, and an appropriate amount of deionized water was added to adjust the concentration of the obtained aramid nanofiber solution to 10 mg / g.

[0075] (2) Preparation of carbon nanotube / aramid nanofiber aerogel:

[0076] 16g of ANF solution was placed in a homemade 4*4*2cm mold, and 0.032g of carbon nanotubes was added. After stirring evenly, the sample was frozen at -40°C and then freeze-dried for 120h to obtain CNTs / ANF aerogel ( Figure 4 ).

[0077] Effect test

[0078] The samples of Examples 1, 2, 3 and Comparative Example 1 were cut into rectangular blocks with a size of 22.84 mm × 10.13 mm, and the variable temperature electromagnetic parameters of different aerogels were tested in the X-band (8.2-12.4 GHz) by the waveguide method in a high temperature waveguide test fixture Ceyear vector network analyzer with an in-situ heating platform.

[0079] Test results:

[0080] It can be seen from Figures 6 to 9 that in the X-band, the real and imaginary parts of the dielectrics of the samples in Examples 1 to 3 of the present invention change significantly compared to those in Comparative Example 1, and increase as the temperature rises.

[0081] exist Fig.10 In the wave absorption performance obtained by calculation, it is found that Example 1 has the function of real-time tunable frequency as the temperature rises. Example 2 has a switchable function of wave absorption performance from off to on. Example 3 has a switchable function of wave absorption performance from on to off. The realization of the two functions of frequency tunability and wave absorption switchability of Examples 1-3 is mainly attributed to the phase change behavior produced by different contents of vanadium dioxide, which will bring different degrees of interface polarization effect with other various interfaces, and cooperate with various loss mechanisms to adjust impedance matching and attenuation constants to achieve the above functions.

[0082] The present invention provides a temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel and a preparation method thereof. First, vanadium dioxide filler with adjustable dielectric properties is prepared, and then it is synthesized in a certain proportion after being modified with carbon nanotubes respectively, and then added to a hydrogel with aramid nanofibers as a skeleton and freeze-dried to obtain CNTs / VO with intelligent dynamic adjustable dielectric properties. 2 / ANF composite aerogel. The frequency-adjustable and wave-absorbing switchable aerogel prepared by the preparation method of the present invention is tested by the vector network analyzer waveguide method variable temperature test. We can see that compared with the aerogel without adding vanadium dioxide, the real and imaginary parts of its dielectric constant are much smaller than those of the aerogel with added vanadium dioxide, and the change with temperature is not obvious, indicating that the introduction of vanadium dioxide increases the dielectric constant and the degree of its change with temperature. In addition, the aerogel with aramid nanofiber as the skeleton has a porous structure, which makes it easier for electromagnetic waves to enter the interior of the material for attenuation. The present invention provides insights into intelligent electromagnetic wave absorption performance and opens the way for the intelligent control application of electromagnetic absorbers driven by temperature.

[0083] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel. It is characterized in that include: The vanadium dioxide powder is surface modified to obtain vanadium dioxide with amino functional groups on the surface; The vanadium dioxide with amino functional groups on the surface is compounded with carboxylated carbon nanotubes to obtain a wave absorbing filler; the wave absorbing filler is evenly mixed with the aramid nanofiber dispersion and then freeze-dried to obtain CNTs / VO 2 / ANF hybrid aerogel; The method for surface modification of vanadium dioxide powder is as follows: vanadium dioxide is mixed with anhydrous ethanol and ultrasonically treated, and then APTES is added, magnetically stirred, and then centrifuged to obtain vanadium dioxide with amino functional groups on the surface; The composite method of vanadium dioxide with amino functional groups on the surface and carboxyl carbon nanotubes is as follows: vanadium dioxide with amino functional groups on the surface and carboxyl carbon nanotubes are mixed in water, magnetically stirred in a water bath, and then washed and dried to obtain a wave absorbing filler.

2. The method for preparing the temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel according to claim 1, It is characterized in that The freeze-drying temperature is -50~-30℃.

3. The method for preparing the temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel according to claim 1, It is characterized in that The ratio of the carboxylated carbon nanotubes, the vanadium dioxide with amino functional groups on the surface and the aramid nanofiber dispersion is (0.024-0.040) g: (0.072-0.120) g: 16 g; In the aramid nanofiber dispersion, the mass concentration of aramid nanofiber is 9-11 mg / g.

4. The method for preparing the temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel according to claim 1, It is characterized in that The ratio of the carboxylated carbon nanotubes, the vanadium dioxide with amino functional groups on the surface and the aramid nanofiber dispersion is (0.024-0.040) g: (0.120-0.200) g: 16 g; In the aramid nanofiber dispersion, the mass concentration of aramid nanofiber is 9-11 mg / g.

5. The method for preparing the temperature-driven intelligent adjustable electromagnetic wave absorbing composite aerogel according to claim 1, It is characterized in that The ratio of the carboxylated carbon nanotubes, the vanadium dioxide with amino functional groups on the surface and the aramid nanofiber dispersion is (0.072-0.088) g: (0.360-0.440) g: 16 g; In the aramid nanofiber dispersion, the mass concentration of aramid nanofiber is 9-11 mg / g.

6. An aerogel with adjustable wave absorption frequency prepared according to the preparation method of claim 3.

7. An aerogel with switchable wave absorbing function prepared according to the preparation method of claim 4.

8. An aerogel with switchable wave absorbing function prepared according to the preparation method of claim 5.