A thermally conductive composite material and its preparation method and application

By precisely controlling silicone oil raw materials and fillers and optimizing cross-linking density and conversion rate, the problems of short service life and performance changes of silicone thermally conductive composite materials at high temperatures are solved, and the long-term stability of thermally conductive composite materials at high temperatures is achieved. and high performance.

CN117986872BActive Publication Date: 2024-10-18SHENZHEN JINGTU MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310597730.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-10-18
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

Existing silicone thermally conductive composite materials have a short service life and obvious performance changes at high temperatures, and the filling of thermally conductive powder affects the curing speed and cross-linking density of silicone rubber, resulting in a decrease in thermal stability, making it difficult to simultaneously take into account thermal conductivity, shape stability and Mechanical properties.

Method used

Through precise control of silicone oil raw materials, proportions and curing conditions, we use high-viscosity vinyl-terminated silicone oil, hydrogen-containing silicone oil, platinum catalyst and modified alumina filler, combined with silane coupling agent treatment, to optimize cross-linking density and conversion rate , reduce the volatilization and side reactions of low molecular substances, and improve the high-temperature stability of thermally conductive composite materials.

Benefits of technology

The prepared thermally conductive composite material has stable performance in the range of 200~250℃, with a thermal conductivity coefficient of 2~4W/m·K, a compression rebound rate of up to 95%, and a performance change rate of less than 15% after more than 1 to 3 years of use. , significantly improving the high-temperature stability of the material's chemical and physical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a thermally conductive composite material and its preparation method and application. The thermally conductive composite material comprises: 80 to 200 parts by mass of high-viscosity vinyl-terminated silicone oil; 0.7 to 3 parts by mass of hydrogen-containing silicone oil; 1 to 10 parts by mass of low-viscosity vinyl-terminated silicone oil; 0.15 to 0.3 parts by mass of inhibitor; 0.1 to 0.2 parts by mass of platinum catalyst; 800 to 1000 parts by mass of thermally conductive filler; the thermally conductive filler is ① an alumina filler with a surface oxygen-aluminum element mass ratio of 1.1 to 1.4 or ② an alumina filler with a surface oxygen-aluminum element ratio of 1.1 to 1.4 and treated with a silane coupling agent. The present invention aims at the problem that the thermally conductive silicone material has poor thermal stability above 200°C or in long-term use. By compounding silicone oil and thermally conductive filler, a thermally conductive composite material with a change rate of less than 15% in parameters such as shore00 hardness, compression rebound rate, and thermal conductivity coefficient during long-term use at 200 to 250°C is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermal interface materials, and in particular to a thermally conductive composite material and a preparation method and application thereof. Background Art

[0002] Silicone rubber is usually obtained by cross-linking and curing low molecular weight vinyl dimethyl polysiloxane, and can be divided into addition-type silicone and dealcohol-type silicone according to the different cross-linking methods. Since the bond energy of silicon-oxygen bonds is higher than that of carbon-carbon bonds and it is easier to rotate internally, the elasticity, weather resistance and other properties of silicone materials are better than most natural rubbers and synthetic resins, so they are often used in high temperature, elastic filling and other scenarios. Due to the low thermal conductivity of polymer materials themselves, thermally conductive and insulating powder materials such as aluminum oxide, aluminum nitride, zinc oxide, and boron nitride are generally filled into silicone materials to prepare thermally conductive and insulating filling materials for electronic packaging to achieve protection of precision components and heat transfer effects. However, the filling of thermally conductive powders will affect the curing speed and cross-linking density of silicone rubber, which will reduce the thermal stability of silicone rubber.

[0003] Most silicone thermally conductive composite materials cannot be used for a long time at temperatures above 200°C, or have problems such as short service life and obvious performance changes in thermally conductive application scenarios. Therefore, it is of great significance to develop silicone thermally conductive composite materials with high thermal stability. At present, there are two main methods to improve the heat resistance of silicone materials. One is to introduce aromatic groups with higher thermal stability, and the other is to add additives to inhibit side reactions. Patents CN101356214A and CN108587454A introduce aromatic groups into silicone resins to maintain high light transmittance for a long time at 200°C, but the preparation process of polysiloxane containing benzene rings is more complicated and is usually used in the LED industry. Patent CN101627046A adds a new type of thermal stabilizer to prepare a silicone elastomer that still maintains the fracture strength, elasticity and hardness that meet the use requirements after 7 days at 250°C. Patent CN105131606A adds antioxidants to silicone rubber to improve its high temperature resistance by 40%, but no corresponding testing process is provided. Patent CN113698912A introduces cerium complexes into silicone, which can keep the mechanical properties and light transmittance of silicone rubber at 250°C, and is used for LED packaging. Patent CN115491171A uses silicon micropowder to enhance the heat resistance of thermally conductive silicone potting glue, and can maintain the bonding performance after 24h treatment at 300°C. The above method can inhibit the aging of silicone rubber caused by side reactions and degradation to a certain extent, but within the range of 200-300°C, degradation is not the only factor affecting the thermal stability of silicone. Low molecular weight group analysis, volatilization, re-crosslinking, curing reaction conversion rate, etc. will also affect the product shape, hardness, elasticity and other properties.

[0004] Thermally conductive silicone rubber composite materials used for electronic packaging need to take into account thermal conductivity, shape stability, mechanical stability, heat resistance, etc., and a deeper understanding of the aging mechanism of silicone composite materials is needed. According to experimental results, there are many phenomena in the aging process of silicone materials, such as degradation, volatilization, change in cross-linking density, end group decomposition, and pumping out. These phenomena affect the long-term performance of silicone thermal conductive materials to varying degrees. Therefore, it is necessary to improve the heat resistance of thermally conductive silicone materials from multiple aspects such as raw materials, formulas, additives, and processes. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a thermally conductive composite material and a preparation method and application thereof. By precisely controlling the silicone oil raw materials, proportions, and curing conditions, the crosslinking density control and high conversion rate are achieved, and the instability of the thermal conductivity, shape, and mechanical properties of the organic silicon thermally conductive composite material caused by the volatilization of low molecular weight substances, side reactions, and re-crosslinking under long-term high temperature conditions is reduced.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] In one aspect, the present invention provides a thermally conductive composite material, comprising:

[0008] 80 to 200 parts by mass of high viscosity vinyl-terminated silicone oil;

[0009] 0.7-3 parts by mass of hydrogen-containing silicone oil;

[0010] 1 to 10 parts by weight of low-viscosity vinyl-terminated silicone oil;

[0011] 0.15-0.3 parts by mass of inhibitor;

[0012] 0.1-0.2 parts by mass of platinum catalyst;

[0013] 800-1000 parts by mass of thermally conductive filler;

[0014] The thermal conductive filler is ① an alumina filler having a surface oxygen-aluminum element mass ratio of 1.1 to 1.4 or ② an alumina filler having a surface oxygen-aluminum element ratio of 1.1 to 1.4 and treated with a silane coupling agent.

[0015] As a preferred embodiment, the silicon content on the surface of the alumina filler is 0-5%.

[0016] In the technical solution of the present invention, after being treated with a silane coupling agent, part of the silane is grafted onto the surface of the alumina filler, and the silane coupling agent is selected from at least one of a vinyl silane coupling agent, an alkoxy silane coupling agent and a glycidyloxypropyl silane coupling agent.

[0017] In the technical solution of the present invention, the oxygen-to-aluminum element ratio and silicon element content of the modified alumina surface are measured by an XPS photoelectron spectrometer, specifically the element composition and content at a depth not exceeding 10 nm, where the Si element content is a mass fraction.

[0018] As a preferred embodiment, the mass percentage of the thermally conductive filler based on the thermally conductive composite material is ≥90%, and the thermally conductive filler is an aluminum oxide filler having a surface oxygen-aluminum element ratio of 1.1 to 1.4 and treated with a silane coupling agent.

[0019] As a preferred embodiment, the surface oxygen-aluminum ratio of 1.1 to 1.4 is obtained by at least one of calcination and vacuum heat treatment, preferably vacuum heat treatment; in the technical solution of the present invention, the calcination process is carried out in an aerobic environment, the chemical reaction of the surface functional groups is complex, and the surface element composition and content cannot be controlled, while vacuum heat treatment can significantly reduce the surface oxygen content;

[0020] Preferably, the temperature of the vacuum heat treatment is 500-900° C., the time is 1-2 hours, and the vacuum degree is not less than -0.09 MPa.

[0021] As a preferred embodiment, the particle size of the thermally conductive filler is 0.5 to 60 μm;

[0022] Preferably, the thermally conductive filler is compounded according to a mass ratio of 0.5-0.9 μm: 1-10 μm: 40-60 μm of particle size of 0-3: 10-40: 50-90.

[0023] As a preferred embodiment, the viscosity of the high-viscosity vinyl-terminated silicone oil is 1000-10000 mPa·s, and the vinyl content is 0.01%-0.32%;

[0024] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 0.6% to 1%;

[0025] Preferably, the viscosity of the low-viscosity vinyl-terminated silicone oil is 100 to 500 mPa·s, and the vinyl content is 0.4% to 1.0%.

[0026] In certain specific embodiments, the inhibitor is selected from at least one of acetylene alcohol inhibitors, but is not limited thereto.

[0027] On the other hand, the present invention provides a method for preparing the above-mentioned thermally conductive composite material, comprising the steps of impregnating the thermally conductive filler with a mixture of high-viscosity terminal vinyl silicone oil and hydrogen-containing silicone oil, diluting the platinum catalyst and inhibitor with low-viscosity terminal vinyl silicone oil and adding the above-mentioned mixture, and heating and curing after mixing the components.

[0028] As a preferred embodiment, the temperature of the heating and curing is 100 to 140° C., and the time of the heating and curing is 5 to 30 minutes.

[0029] In another aspect, the present invention provides use of the thermally conductive composite material in electronic packaging, specifically, use in preparing a thermally conductive gasket.

[0030] In the technical solution of the present invention, the thermally conductive composite material prepared by the above method can be cut to obtain a thermally conductive gasket, the hardness of the thermally conductive gasket is shore 00 or shore A level, the thermal conductivity is 2 to 4 W / m·K, the compression rebound rate can reach up to 95%, and after being used at 200 to 250°C for more than 1 to 3 years, the change rate of the above performance indicators is less than 15%.

[0031] The above technical solution has the following advantages or beneficial effects:

[0032] The thermally conductive composite material provided by the present invention is cross-linked by the reaction of active functional groups during the synthesis process, so that the system has certain elasticity and strength. The silicon-oxygen bond in the silicone oil has a high bond energy and has high chemical stability at high temperatures. The present invention controls the balance between the reaction activity and the curing time of the system by surface modification of the thermally conductive filler and optimizing the ratio between different components, thereby improving the conversion rate during the cross-linking and curing process, so that the thermally conductive composite material can maintain stable chemical and physical properties for a long time at high temperatures. DETAILED DESCRIPTION

[0033] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0034] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0035] Comparative Example 1

[0036] 100g of aluminum oxide with an average particle size of 65μm and a surface oxygen-aluminum ratio of 1.5 and a silicon content of 0% (characterized by XPS photoelectron spectrometer, the same as in the following examples) was added to 14g of vinyl-terminated silicone oil with a viscosity of 1000mPa·s (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully infiltrate; 6g of hydrogen-containing silicone oil with a hydrogen content of 0.75% (Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) was added;

[0037] 0.015 g of platinum catalyst and 0.02 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0038] Curing at 130°C for 15 minutes to obtain a thermally conductive gasket.

[0039] The thermal conductivity of the thermally conductive pad prepared in this comparative example is 1.6W / m·K, and the shore 00 hardness is 90 (the thickness of the test sample is 6mm, and the following examples use the same test method). After the thermally conductive pad is heat-treated at 250°C for 24 hours, the hardness of the thermally conductive pad changes by 300%, the mass loss of the organic silicon component exceeds 5% (the mass difference before and after the heat treatment is measured by weighing method relative to the mass of the sample), and the compression rebound rate after heat treatment is 30% (the test method for the rebound rate is to heat-treat a 25mm×25mm×2mm sample at a compression amount of 50%, and record the rebound amount for 30 minutes after the pressure is released. The following examples use the same test method).

[0040] Example 1

[0041] 100g of alumina with an average particle size of 10μm and a surface oxygen-aluminum ratio of 1.36 and a silicon content of 0% was fully infiltrated into 16g of vinyl-terminated silicone oil with a viscosity of 5000mPa·s (vinyl content of 0.18%, Runhe New Materials Co., Ltd.); 0.3g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0042] 0.015 g of platinum catalyst and 0.02 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0043] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0044] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 1.3 W / m·K, the shore 00 hardness is 60, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250°C for 24 hours is 30%, the mass loss of the silicone component does not exceed 2%, and the compression rebound rate after heat treatment is 90%.

[0045] Example 2

[0046] Alumina with a surface oxygen-aluminum ratio of 1.36 and a silicon content of 0% was compounded according to the mass of 50g and 30g of particle sizes of 60μm and 10μm, respectively, and added to a mixture of 15g of vinyl-terminated silicone oil with a viscosity of 5000mPa·s (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 5g of vinyl-terminated silicone oil with a viscosity of 1000mPa·s (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and fully dispersed; 0.1g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0047] 0.015 g of platinum catalyst and 0.02 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0048] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0049] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 2.4 W / m·K, the shore 00 hardness is 70, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 20%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 90%.

[0050] Example 3

[0051] Alumina with a surface oxygen-aluminum ratio of 1.36 and a silicon content of 0% was compounded according to the mass of 70g and 20g of particle sizes of 60μm and 10μm, respectively, and added to a mixture of 9g of vinyl-terminated silicone oil with a viscosity of 5000mPa·s (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 1g of vinyl-terminated silicone oil with a viscosity of 1000mPa·s (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully infiltrate; 0.1g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0052] 0.015 g of platinum catalyst and 0.02 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0053] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0054] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 2.7 W / m·K, the shore 00 hardness is 70, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 10%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 95%.

[0055] Example 4

[0056] The surface oxygen-aluminum ratio is 1.36, and the silicon content is 0%. The mass of the particles with a particle size of 60 μm and 10 μm is 70 g and 20 g respectively, and added to a mixture of 9 g of a vinyl-terminated silicone oil with a viscosity of 5000 mPa·s (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 1 g of a vinyl-terminated silicone oil with a viscosity of 1000 mPa·s (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully infiltrate; 0.08 g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) is added;

[0057] 0.02 g of platinum catalyst and 0.03 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0058] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0059] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 2.7 W / m·K, the shore 00 hardness is 65, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 5%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 95%.

[0060] Example 5

[0061] Alumina with a surface oxygen-alumina ratio of 1.36 was compounded according to the mass of 75g, 12g and 3g of particle sizes of 60μm, 10μm and 500nm respectively, and then a silane coupling agent was grafted on the surface. The specific operation was to hydrolyze 0.3g of vinyltrimethoxysilane in 20mL of a mixed solvent of water and ethanol in a volume ratio of 7:3 for 1h, then add the above-mentioned aluminum oxide and treat it at 60℃ for 1h, then wash with deionized water, filter and dry, so that the silicon content on the surface of the aluminum oxide is 0.7%;

[0062] The above aluminum oxide was added to a mixture of 7 g of 5000 mPa·s vinyl-terminated silicone oil (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 1 g of 1000 mPa·s vinyl-terminated silicone oil (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully wet; 0.07 g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0063] 0.02 g of platinum catalyst and 0.03 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0064] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0065] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 3.5 W / m·K, the shore 00 hardness is 80, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 5%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 90%.

[0066] Example 6

[0067] Alumina with a surface oxygen-aluminum ratio of 1.36 was compounded according to the mass of 75g, 12g and 3g of particle size 60μm, 10μm and 500nm respectively, and added to a mixture of 7g of terminal vinyl silicone oil with a viscosity of 5000mPa·s (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 1g of terminal vinyl silicone oil with a viscosity of 1000mPa·s (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully infiltrate; 0.07g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0068] 0.02 g of platinum catalyst and 0.03 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0069] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0070] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 3.1 W / m·K, the shore 00 hardness is 85, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250°C for 24 hours does not exceed 5%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 90%.

[0071] Example 7

[0072] Alumina with a surface oxygen-aluminum ratio of 1.36 was compounded according to the particle sizes of 60 μm, 10 μm, and 500 nm, with the masses of 75 g, 12 g, and 3 g, respectively, and then dried at 700°C and a vacuum degree of -0.09 MPa for 2 hours to make the surface oxygen-aluminum ratio of 1.2;

[0073] The above aluminum oxide was added to a mixture of 9 g of 5000 mPa·s vinyl-terminated silicone oil (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 1 g of 1000 mPa·s vinyl-terminated silicone oil (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully wet the mixture; 0.1 g of hydrogen-containing silicone oil (Runhe New Materials Co., Ltd.) with a hydrogen content of 0.81% was added;

[0074] 0.02 g of platinum catalyst and 0.03 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0075] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0076] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 3.0 W / m·K, the shore 00 hardness is 70, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 5%, the mass loss of the silicone component does not exceed 0.5%, and the compression rebound rate after heat treatment is 95%.

[0077] Example 8

[0078] Alumina with a surface oxygen-aluminum ratio of 1.36 was compounded according to the mass of 75g, 12g and 3g of particle size 60μm, 10μm and 500nm respectively, and then a silane coupling agent was grafted on the surface (the method is the same as that of Example 5) to make the silicon content of the surface of the alumina 0.7%, and then added to a mixture of 4.5g of vinyl-terminated silicone oil with a viscosity of 5000mPa·s (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 0.5g of vinyl-terminated silicone oil with a viscosity of 1000mPa·s (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully infiltrate; 0.02g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0079] 0.02 g of platinum catalyst and 0.03 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0080] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0081] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 4 W / m·K, the shore 00 hardness is 95, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 5%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 80%.

[0082] Example 9

[0083] Alumina with a surface oxygen-aluminum ratio of 1.36 was compounded according to the mass of 75g, 12g and 3g of particle size 60μm, 10μm and 500nm respectively, and added to a mixture of 4.5g of 5000mPa·s vinyl-terminated silicone oil (vinyl content of 0.18%, Runhe New Materials Co., Ltd.) and 0.5g of 1000mPa·s vinyl-terminated silicone oil (vinyl content of 0.32%, Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) to fully infiltrate; 0.02g of hydrogen-containing silicone oil with a hydrogen content of 0.81% (Runhe New Materials Co., Ltd.) was added;

[0084] 0.02 g of platinum catalyst and 0.03 g of 2-methyl-3-butyn-2-ol (inhibitor) were diluted with 1 g of low-viscosity vinyl-terminated silicone oil (vinyl content of 0.56%, viscosity of 300 mPa·s, purchased from Shenzhen Jipeng Silicon Fluoride Chemical Co., Ltd.) and added to the above reaction system;

[0085] Curing at 130° C. for 20 min gave a thermally conductive gasket.

[0086] Tests show that the thermal conductivity of the thermally conductive gasket prepared in this embodiment is 4.3 W / m·K, the shore 00 hardness is 90, the hardness change of the thermally conductive silicone rubber sheet after heat treatment at 250° C. for 24 hours does not exceed 5%, the mass loss of the silicone component does not exceed 1.5%, and the compression rebound rate after heat treatment is 10%.

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A thermally conductive composite material, characterized in that: include: 80 to 200 parts by mass of high-viscosity vinyl-terminated silicone oil; the viscosity of the high-viscosity vinyl-terminated silicone oil is 1000 to 10000 mPa·s; 0.7~3 parts by mass of hydrogen-containing silicone oil; 1 to 10 parts by weight of low-viscosity vinyl-terminated silicone oil; the viscosity of the low-viscosity vinyl-terminated silicone oil is 100 to 500 mPa·s; 0.15~0.3 parts by mass of inhibitor; 0.1~0.2 parts by mass of platinum catalyst; 800~1000 parts by mass of thermal conductive filler; The thermal conductive filler is ① an alumina filler having a surface oxygen-aluminum element mass ratio of 1.1 to 1.4 or ② an alumina filler having a surface oxygen-aluminum element mass ratio of 1.1 to 1.4 and treated with a silane coupling agent.

2. The thermally conductive composite material according to claim 1, characterized in that: The silicon content on the surface of the alumina filler is 0-5%.

3. The thermally conductive composite material according to claim 1, characterized in that: The silane coupling agent is selected from at least one of a vinyl silane coupling agent, an alkoxy silane coupling agent and a glycidyloxypropyl silane coupling agent.

4. The thermally conductive composite material according to claim 1, characterized in that: The mass percentage of the thermally conductive filler based on the thermally conductive composite material is ≥90%, and the thermally conductive filler is an aluminum oxide filler with a surface oxygen-aluminum element mass ratio of 1.1-1.4 and treated with a silane coupling agent.

5. The thermally conductive composite material according to claim 1, characterized in that: The surface oxygen-aluminum element mass ratio of 1.1 to 1.4 is obtained by at least one of calcination and vacuum heat treatment.

6. The thermally conductive composite material according to claim 5, characterized in that: The surface oxygen-aluminum element mass ratio is 1.1-1.4 and is obtained by vacuum heat treatment.

7. The thermally conductive composite material according to claim 6, characterized in that: The temperature of the vacuum heat treatment is 500-900°C, the time is 1-2 h, and the vacuum degree is not less than -0.09 MPa.

8. The thermally conductive composite material according to claim 1, characterized in that: The particle size of the thermal conductive filler is 0.5-60 μm.

9. The thermally conductive composite material according to claim 8, characterized in that: The thermal conductive filler is compounded according to a mass ratio of 0.5-0.9 µm: 1-10 µm: 40-60 µm of particle size of 0-3: 10-40: 50-90.

10. The thermally conductive composite material according to claim 1, characterized in that: The high-viscosity vinyl-terminated silicone oil has a vinyl content of 0.01% to 0.32%.

11. The thermally conductive composite material according to claim 1, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 0.6% to 1%.

12. The thermally conductive composite material according to claim 1, characterized in that: The vinyl content of the low-viscosity vinyl-terminated silicone oil is 0.4% to 1.0%.

13. The method for preparing the thermally conductive composite material according to any one of claims 1 to 12, characterized in that: The method comprises the steps of impregnating the thermal conductive filler with a mixture of high-viscosity vinyl-terminated silicone oil and hydrogen-containing silicone oil, diluting the platinum catalyst and inhibitor with low-viscosity vinyl-terminated silicone oil and adding the mixture, and heating and curing after mixing the components.

14. The preparation method according to claim 13, characterized in that: The temperature of the heating and curing is 100-140° C., and the time of the heating and curing is 5-30 min.

15. Use of the thermally conductive composite material according to any one of claims 1 to 12 in electronic packaging, characterized in that: Use in the preparation of thermally conductive pads.

Citation Information

Patent Citations

  • Thermally stable transparent silicone resin compositions and methods for their preparation and use

    CN101356214A

  • Thermally-stable hot cross-linking elastomer silicone composition

    CN101627046A

  • Method for improving heat resistance of silica gel

    CN105131606A

  • High-temperature-resistance, anti-aging and high-transparent organic silica gel

    CN108587454A

  • High-temperature-aging-resistant packaging silica gel as well as preparation method and application thereof

    CN113698912A