Aluminum alloy modifier and aluminum alloy modification treatment method

Through the aluminum alloy deterioration agent formula without strontium element and specific treatment methods, the metallographic structure of silicon-aluminum alloy is refined, and the problems of pore formation and performance reduction are solved, and better mechanical properties and denseness are achieved.

CN117987678BActive Publication Date: 2024-11-08XUZHOU SI YUAN ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410235587.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-01
Publication Date
2024-11-08
Estimated Expiration
2044-03-01

AI Technical Summary

Technical Problem

While improving the mechanical properties of the alloy, the existing silicon-aluminum alloy deterioration agents are prone to cause pore formation and affecting density. The large-scale introduction of P elements will reduce the performance of aluminum alloys, and the existing deterioration agents have limited effects.

Method used

Using a aluminum alloy deteriorator formula without strontium elements, NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium intermediate alloy and aluminum-phosphorus intermediate alloy, combined with trace phosphorus elements, refined eutectic silicon by slow cooling and stirring treatment and primary silicon structure to avoid pore formation.

Benefits of technology

Effectively refine the metallographic structure of silicon-aluminum alloy, improve its mechanical properties, ensure the density and crack resistance of the ingot, which is better than the traditional metamorphic agent treatment effect containing strontium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117987678B_ABST
    Figure CN117987678B_ABST
Patent Text Reader

Abstract

The present application discloses an aluminum alloy modifier and an aluminum alloy modification treatment method. On the one hand, the present application provides an aluminum alloy modifier for modification treatment of silicon aluminum alloy with a silicon content of 12 to 30%. The components of the aluminum alloy modifier include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 10 to 20%, the content of KCl is 10 to 20%, the content of NF is 5 to 10%, the content of KBF4 is 10 to 20%, the content of cerium is 8 to 10%, and the content of phosphorus is 0.2 to 0.4%. On the other hand, the present application also provides an aluminum alloy modification treatment method using the above-mentioned aluminum alloy modifier. The present application can better modify the silicon aluminum alloy, effectively refine the metallographic structure of the silicon aluminum alloy, and effectively improve the various mechanical properties of the silicon aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum alloy casting, and in particular to an aluminum alloy modifier and an aluminum alloy modification treatment method, which are mainly suitable for vacuum heat treatment of titanium alloys and parts with specific requirements. Background Art

[0002] Aluminum is the most commonly used metal among nonferrous metals. Due to its low density, high specific strength, and excellent electrical and thermal conductivity, it is widely used in various aspects of life and production, such as transportation, machinery, aerospace, chemical industry, and building materials. At present, cast aluminum alloy materials are widely used, and cast silicon aluminum alloy materials are the largest and most widely used cast aluminum alloy materials. Silicon with a relatively small density is added to the silicon aluminum alloy, and the overall density is low, and the cost is also low, but it has good thermal conductivity, high specific strength and rigidity, good plating performance with gold, silver, copper, and nickel, can be welded with the substrate, and is easy for precision machining. With the increase of the silicon content in the silicon aluminum alloy, the density and thermal expansion coefficient of the alloy material can be significantly reduced, and the heat resistance and corrosion resistance of the alloy can also be improved.

[0003] However, silicon-aluminum alloys also have certain defects. The number of eutectics in the alloy will increase with the increase of silicon addition, and the eutectic silicon structure is in the form of coarse laths or needles without modification. When the silicon content exceeds the eutectic composition, primary silicon will form, generally in the form of coarse polygonal blocks. These coarse and irregular metallographic structures will affect the mechanical properties of the alloy, increase the brittleness of the alloy, reduce the plasticity and cutting performance of the alloy, and thus affect its application.

[0004] In actual production, in order to solve the above problems, silicon aluminum alloys are usually subjected to modification treatment. Modification treatment refers to the addition of a small amount of other elements to the original alloy ingredients in order to improve the metallographic structure to meet certain requirements when smelting the alloy, so that the metallographic microstructure of the alloy is changed to obtain an ideal metallographic structure. In existing actual production, modification treatment is usually carried out by adding a modifier. This treatment method has good effect, low cost and easy operation. The modification mechanism of the modifier is relatively complex, and the existing modifiers are divided into two categories: single element modifiers and composite modifiers. At present, it has been found that elements such as Na, K, Re, Ba, Sr, P, Bi, Sb have a modifying effect on eutectic silicon, and they are usually added to the aluminum alloy melt in the form of pure metals, intermediate alloys and fluxes. The existing various types of modifiers are usually composed of single elements, composite intermediate alloys, or compounds containing the above elements. Among them, the modifiers of P element, Na element and Sr element are the most common. The P element has a significant modifying effect on primary silicon, while the Na and Sr elements have a significant modifying effect on eutectic silicon.

[0005] However, when silicon aluminum alloy is modified, the introduction of a large amount of P element will lead to a decrease in the performance of the aluminum alloy; and the addition of Sr element will cause pores in the silicon aluminum alloy, affecting the compactness, and also leading to a decrease in the performance of the aluminum alloy. Therefore, the field urgently needs to develop a more excellent modifier to improve the modification effect of the existing silicon aluminum alloy. Summary of the invention

[0006] In order to solve at least one of the above technical problems, a modification process is developed that can better modify silicon-aluminum alloys, effectively refine the metallographic structure of silicon-aluminum alloys, and effectively improve the mechanical properties of silicon-aluminum alloys. The present application provides an aluminum alloy modifier and an aluminum alloy modification method.

[0007] On the one hand, the present application provides an aluminum alloy modifier for the modification treatment of a silicon aluminum alloy with a casting silicon content of 12 to 30%, wherein the components of the aluminum alloy modifier include NaCl, KCl, NF, KBF4, pure aluminum, an aluminum-cerium master alloy and an aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 10 to 20%, the content of KCl is 10 to 20%, the content of NF is 5 to 10%, the content of KBF4 is 10 to 20%, the content of cerium is 8 to 10%, and the content of phosphorus is 0.2 to 0.4%.

[0008] Optionally, the aluminum alloy modifier further includes an aluminum-yttrium master alloy, and the content of yttrium in the aluminum alloy modifier is 0.5-1% by weight.

[0009] Optionally, the aluminum-cerium master alloy is in the form of powder, and the particle size of the powder is 150 to 600 μm.

[0010] Optionally, the aluminum-strontium master alloy is in the form of powder, and the particle size of the powder is 150 to 600 μm.

[0011] Optionally, the aluminum-phosphorus master alloy is in the form of powder, and the particle size of the powder is 150 to 600 μm.

[0012] Optionally, the aluminum alloy modifier further comprises graphite powder, and the content of the graphite powder in the aluminum alloy modifier is 1 to 3% by weight.

[0013] On the other hand, the present application also provides a method for modifying an aluminum alloy, using the above-mentioned aluminum alloy modifying agent, comprising the following steps:

[0014] S1. Adding silicon-aluminum alloy raw materials into a smelting furnace, heating to 860-920° C., keeping warm for 15-30 minutes under an inert gas atmosphere, sampling and testing, and adjusting the composition to obtain silicon-aluminum alloy liquid;

[0015] S2, adding an aluminum alloy modifier to the silicon-aluminum alloy liquid obtained in step S1 at a temperature of 860-920° C. in a proportion of 4-6% of the total weight of the silicon-aluminum alloy liquid, and stirring the mixture under an inert gas atmosphere for 10-15 minutes to obtain an alloy solution;

[0016] S3, cooling the alloy solution obtained in step S2 to 740-760° C. at a cooling rate of 4-6° C. / min under stirring under an inert gas atmosphere, and then keeping the temperature and stirring for 30-45 minutes, and then keeping the temperature and standing for 15-20 minutes to obtain a silicon-aluminum alloy liquid that has been modified;

[0017] S4, casting the modified silicon-aluminum alloy liquid obtained in step S3.

[0018] Optionally, in step S1, the heating temperature is controlled at 880-900°C.

[0019] Optionally, in steps S1 to S3, the inert gas is argon.

[0020] Optionally, in step S4, the casting temperature is controlled at 700-720°C, and the cooling rate is not less than 10 6 K / S.

[0021] In summary, the present invention includes at least one of the following beneficial technical effects:

[0022] 1. The present application designs an aluminum alloy modifier, which is designed for the modification of silicon-aluminum alloys with medium and high silicon contents. The aluminum alloy modifier of the present application adopts a formula design that does not contain strontium elements, uses cerium elements in combination with NF and KBF4 as the main components of the modifier, and adds a trace amount of phosphorus elements. It can effectively refine the metallographic structure of the silicon-aluminum alloy during the modification of silicon-aluminum alloys with medium and high silicon contents, avoid the formation of coarse eutectic silicon structure and primary silicon structure, and effectively improve the various mechanical properties of silicon-aluminum alloy ingots.

[0023] 2. The present application also designs a treatment method for the modification of silicon-aluminum alloys with medium and high silicon contents based on the aluminum alloy modifier of the present application. The treatment method of the present application has simple steps, and the growth of eutectic silicon structure and primary silicon structure is controlled by initially slowly cooling the temperature in combination with the aluminum alloy modifier of the present application, and then the eutectic silicon structure and primary silicon structure are refined through stirring and heat preservation treatment. The mechanical properties of the silicon-aluminum alloy ingot obtained by the modification treatment method of the present application are all excellent.

[0024] 3. In the aluminum alloy modifier and modification treatment method of the present application, strontium element is not introduced, which effectively avoids the generation of pores in the aluminum alloy during the treatment and casting process. The obtained silicon aluminum alloy ingot has better density and excellent crack resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the metallographic structure diagram of the ingot prepared in Comparative Example 1 of the present application;

[0026] Figure 2 This is the metallographic structure diagram of the ingot prepared in Example 1 of the present application;

[0027] Figure 3 This is the metallographic structure diagram of the ingot prepared in Comparative Example 2 of the present application;

[0028] Figure 4 This is the metallographic structure diagram of the ingot prepared in Example 10 of the present application. DETAILED DESCRIPTION

[0029] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0030] The present application designs an aluminum alloy modifier for modification of silicon aluminum alloy with a silicon content of 12 to 30%. The components of the aluminum alloy modifier include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 10 to 20%, the content of KCl is 10 to 20%, the content of NF is 5 to 10%, the content of KBF4 is 10 to 20%, the content of cerium is 8 to 10%, and the content of phosphorus is 0.2 to 0.4%.

[0031] The design of this application adopts a modifier ratio of NF and KBF4 with cerium element, and no strontium element is added. The core purpose is to solve the problem that the strontium element modifier affects the density of aluminum alloy. Since this application is aimed at medium and high content silicon aluminum alloys, a trace amount of phosphorus is added to control the primary silicon structure.

[0032] At present, the modifier containing strontium has excellent modification effect on silicon aluminum alloy, and is the element with the best effect on eutectic silicon structure refinement among the elements used in existing modifiers. However, strontium is extremely active and will form pores in silicon aluminum alloy after use, resulting in a decrease in density, which in turn affects the various properties of silicon aluminum alloy.

[0033] The inventors of the present application adopted a modifier ratio without strontium element, and designed a modifier ratio of NF and KBF4 combined with cerium element. The modification treatment effect of the obtained composite modifier is not inferior to that of the modifier containing strontium element, and effectively avoids the problems of the above-mentioned prior art.

[0034] The present application also provides a method for modifying an aluminum alloy, using the above-mentioned aluminum alloy modifying agent, comprising the following steps:

[0035] S1. Adding silicon-aluminum alloy raw materials into a smelting furnace, heating to 860-920° C., keeping warm for 15-30 minutes under an inert gas atmosphere, sampling and testing, and adjusting the composition to obtain silicon-aluminum alloy liquid;

[0036] S2, adding an aluminum alloy modifier to the silicon-aluminum alloy liquid obtained in step S1 at a temperature of 860-920° C. in a proportion of 4-6% of the total weight of the silicon-aluminum alloy liquid, and stirring the mixture under an inert gas atmosphere for 10-15 minutes to obtain an alloy solution;

[0037] S3, cooling the alloy solution obtained in step S2 to 740-760° C. at a cooling rate of 4-6° C. / min under stirring under an inert gas atmosphere, and then keeping the temperature and stirring for 30-45 minutes, and then keeping the temperature and standing for 15-20 minutes to obtain a silicon-aluminum alloy liquid that has been modified;

[0038] S4, casting the modified silicon-aluminum alloy liquid obtained in step S3.

[0039] The following are specific embodiments of this application:

[0040] The present application example uses a silicon aluminum alloy with a silicon content of 30% as the preparation object. The silicon content is relatively high, greatly exceeding the eutectic composition, and is very easy to form coarse primary silicon structure and eutectic silicon structure. By processing the above object, the technical effect of the present application can be well verified.

[0041] The embodiment of the present application adopts a vacuum melting furnace as the melting equipment, and the raw materials of various components used in the aluminum alloy modifier of the present application are all purchased from the market.

[0042] The silicon-aluminum alloy raw materials of the present application are commercially available pure aluminum ingots and pure silicon ingots. In the embodiments of the present application, argon is used as the inert gas.

[0043] In the aluminum alloy modifiers of Examples 1 to 8 of the present application, each intermediate alloy uses a particle raw material with a particle size of 3 to 5 mm.

[0044] Example 1

[0045] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 10%, the content of KCl is 10%, the content of NF is 5%, the content of KBF4 is 10%, the content of cerium is 8%, and the content of phosphorus is 0.2%.

[0046] The aluminum alloy modification treatment method of this embodiment comprises the following steps:

[0047] S1. Adding silicon-aluminum alloy raw materials into a melting furnace, heating to 920° C., keeping the temperature at 900-920° C. for 30 min under an argon atmosphere, sampling and testing, and adjusting the composition to obtain silicon-aluminum alloy liquid;

[0048] S2, at a temperature of 900-920° C., adding an aluminum alloy modifier to the silicon-aluminum alloy liquid obtained in step S1 at a ratio of 4% of the total weight of the silicon-aluminum alloy liquid, and stirring the mixture under an inert gas atmosphere for 15 minutes to obtain an alloy solution;

[0049] S3, cooling the alloy solution obtained in step S2 to 760° C. at a cooling rate of 4° C. / min under stirring under an inert gas atmosphere, and then keeping the temperature and stirring for 45 min, and then keeping the temperature and standing for 20 min to obtain a silicon-aluminum alloy liquid that has been modified;

[0050] S4, casting the modified silicon-aluminum alloy liquid obtained in step S3, with a casting temperature of 700° C., water cooling, and a cooling rate of 10K / S.

[0051] Example 2

[0052] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 20%, the content of KCl is 20%, the content of NF is 10%, the content of KBF4 is 20%, the content of cerium is 10%, and the content of phosphorus is 0.4%.

[0053] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0054] Example 3

[0055] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0056] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 15%, the content of KCl is 15%, the content of NF is 8%, the content of KBF4 is 15%, the content of cerium is 10%, and the content of phosphorus is 0.3%.

[0057] Example 4

[0058] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 18%, the content of KCl is 18%, the content of NF is 8%, the content of KBF4 is 18%, the content of cerium is 8%, and the content of phosphorus is 0.4%.

[0059] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0060] Example 5

[0061] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy, aluminum-phosphorus master alloy and aluminum-yttrium master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 18%, the content of KCl is 18%, the content of NF is 8%, the content of KBF4 is 18%, the content of cerium is 8%, the content of phosphorus is 0.4%, and the content of yttrium is 0.5%.

[0062] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0063] Example 6

[0064] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy, aluminum-phosphorus master alloy and aluminum-yttrium master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 18%, the content of KCl is 18%, the content of NF is 8%, the content of KBF4 is 18%, the content of cerium is 8%, the content of phosphorus is 0.4%, and the content of yttrium is 1%.

[0065] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0066] Example 7

[0067] The components of the aluminum alloy modifier of this embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy, aluminum-phosphorus master alloy, aluminum-yttrium master alloy and graphite; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 18%, the content of KCl is 18%, the content of NF is 8%, the content of KBF4 is 18%, the content of cerium is 8%, the content of phosphorus is 0.4%, the content of yttrium is 1%, and the content of graphite is 1%.

[0068] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0069] Example 8

[0070] The components of the aluminum alloy modifier of the present embodiment include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy, aluminum-phosphorus master alloy, aluminum-yttrium master alloy and graphite; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 18%, the content of KCl is 18%, the content of NF is 8%, the content of KBF4 is 18%, the content of cerium is 8%, the content of phosphorus is 0.4%, the content of yttrium is 1%, and the content of graphite is 3%.

[0071] This embodiment adopts the same modification treatment method as that of embodiment 1.

[0072] Example 9

[0073] The difference between this embodiment and embodiment 8 is that each intermediate alloy uses a powder raw material with a particle size of 150 to 600 μm.

[0074] Example 10

[0075] The difference between this embodiment and embodiment 9 is that a different modification treatment method is adopted.

[0076] The aluminum alloy modification treatment method of this embodiment comprises the following steps:

[0077] S1. Adding silicon-aluminum alloy raw materials into a melting furnace, heating to 900° C., keeping the temperature at 880-900° C. for 15 minutes under an argon atmosphere, sampling and testing, and adjusting the composition to obtain silicon-aluminum alloy liquid;

[0078] S2, adding an aluminum alloy modifier to the silicon-aluminum alloy liquid obtained in step S1 at a temperature of 880-900° C. in a proportion of 6% of the total weight of the silicon-aluminum alloy liquid, and stirring the mixture under an inert gas atmosphere for 10 minutes to obtain an alloy solution;

[0079] S3, cooling the alloy solution obtained in step S2 to 740° C. at a cooling rate of 6° C. / min under stirring under an inert gas atmosphere, and then keeping the temperature and stirring for 30 min, and then keeping the temperature and standing for 15 min to obtain a silicon-aluminum alloy liquid that has been modified;

[0080] S4, casting the modified silicon aluminum alloy liquid obtained in step S3, the casting temperature is 720°C, water cooling is adopted, and the cooling rate is 10 6 K / S.

[0081] The following is a comparative example of this application

[0082] Comparative Example 1

[0083] This application adopts the embodiment of the Chinese invention patent with publication number CN107460352A as comparative example 1.

[0084] Comparative Example 2

[0085] The difference between this comparative example and Example 10 is that an equal amount of KF is used to replace KBF4 in the aluminum alloy modifier.

[0086] Comparative Example 3

[0087] The difference between this comparative example and Example 10 is that an equal amount of KBF4 is used to replace NaF in the aluminum alloy modifier.

[0088] Comparative Example 4

[0089] The difference between this comparative example and Example 10 is that an equal amount of NaBF4 is used to replace NaF in the aluminum alloy modifier.

[0090] Aluminum alloy ingots were prepared using the methods of Examples 1 to 10 of the present application and Comparative Examples 1 to 4. The silicon aluminum alloy ingot samples prepared in Examples 1 to 10 of the present application and Comparative Examples 1 to 4 were then tested to determine their metallographic structures and comprehensive mechanical properties. The specific test results are shown in Tables 1 and Figures 1 to 4 shown.

[0091] The detection method used in this application is:

[0092] Metallographic structure: Leica DMI 8 optical microscope, Germany;

[0093] Tensile strength (MPa), yield strength (MPa), elongation (%) and impact toughness (KJ / m 2 ): According to the standard "GB / T228.1-2021: Tensile test of metallic materials - Part 1: Room temperature test method", the tensile strength, yield strength, elongation and impact toughness at room temperature are tested.

[0094] Table 1 Mechanical properties test results of ingots of Examples 1 to 10 and Comparative Examples 1 to 4

[0095] performance Tensile strength(MPa) Yield Strength(Mpa) Elongation(%) <![CDATA[Impact toughness (KJ / m 2 )]]> Example 1 352 337 8.6 8.7 Example 2 361 342 8.7 8.9 Example 3 374 356 8.9 9.2 Example 4 378 359 8.9 9.3 Example 5 391 369 9.3 9.9 Example 6 398 372 9.5 10.3 Example 7 401 373 9.5 10.3 Example 8 404 375 9.5 10.4 Example 9 418 387 9.7 11.1 Example 10 426 392 9.8 11.5 Comparative Example 1 272 248 7.1 7.6 Comparative Example 2 266 237 6.9 7.4 Comparative Example 3 261 232 6.4 6.8 Comparative Example 4 257 226 6.3 6.6

[0096] It can be seen from the data in Table 1 that the various mechanical properties of the silicon-aluminum alloy ingots of Examples 1 to 10 of the present application are significantly better than the silicon-aluminum alloy obtained by modification treatment with a strontium-containing aluminum alloy modifier in Comparative Example 1, and are also significantly better than the silicon-aluminum alloys of Comparative Examples 2 to 4. It can be seen that although the aluminum alloy modifier of the present application does not use strontium, the modification effect of the modifier combined with the modification treatment method of the present application is better than the existing modifier containing strontium. In addition, the silicon-aluminum alloys obtained in Examples 1 to 10 of the present application have significantly better impact toughness and elongation than the silicon-aluminum alloy obtained in Comparative Example 1. It can be seen that the silicon-aluminum alloy obtained by the modifier of the present application combined with the modification treatment method of the present application has better compactness and more excellent crack resistance.

[0097] It can also be seen from the data in Table 1 that the various mechanical properties of the silicon-aluminum alloys of Examples 1 to 4 of the present application are significantly different from those of the silicon-aluminum alloys of Examples 5 to 8; the various mechanical properties of the silicon-aluminum alloy of Example 9 of the present application are significantly better than those of the silicon-aluminum alloy of Example 8. It can be seen that after optimizing the particle size of the intermediate alloy of the aluminum alloy modifier of the present application and adding yttrium, the modification effect of the aluminum alloy modifier can be further greatly improved. In addition, the various mechanical properties of the silicon-aluminum alloy of Example 10 of the present application are significantly better than those of the silicon-aluminum alloy of Example 9; it can be seen that after optimizing the process parameters and casting parameters, the performance of the silicon-aluminum alloy can be further improved.

[0098] pass Figure 1 and Figure 2 The comparison, and Figure 3 and Figure 4 By comparing the data in Table 1, it can be seen that after the aluminum alloy modifier of the present application modifies the silicon aluminum alloy, the grain size of the eutectic silicon structure and the primary silicon structure in the silicon aluminum alloy is significantly finer. Figure 3 and Figure 4 , and the data in Table 1 show that the performance of the silicon aluminum alloy of Example 10 of the present application is significantly better than that of the silicon aluminum alloy of Comparative Examples 2 to 4; it can be seen that in the aluminum alloy modifier of the present application, NF, KBF4 and cerium elements have a coordination effect. If this component ratio is not adopted, the modification effect of the modifier will be significantly reduced.

[0099] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. An aluminum alloy modifier, used for the modification of silicon aluminum alloy with a silicon content of 12-30%, characterized in that: The components of the aluminum alloy modifier include NaCl, KCl, NF, KBF4, pure aluminum, aluminum-cerium master alloy and aluminum-phosphorus master alloy; in the aluminum alloy modifier, by weight percentage, the content of NaCl is 10-20%, the content of KCl is 10-20%, the content of NF is 5-10%, the content of KBF4 is 10-20%, the content of cerium is 8-10%, and the content of phosphorus is 0.2-0.4%.

2. The aluminum alloy modifier according to claim 1, characterized in that: The aluminum alloy modifier also includes an aluminum-yttrium master alloy. In the aluminum alloy modifier, the content of yttrium element is 0.5-1% by weight.

3. The aluminum alloy modifier according to claim 1, characterized in that: The aluminum-cerium master alloy is made of powder, and the particle size of the powder is 150-600 μm.

4. The aluminum alloy modifier according to claim 1, characterized in that: The aluminum-phosphorus master alloy is made of powder, and the particle size of the powder is 150-600 μm.

5. The aluminum alloy modifier according to claim 1, characterized in that: The aluminum alloy modifier further comprises graphite powder. In the aluminum alloy modifier, the content of the graphite powder is 1-3% by weight.

6. A method for modifying an aluminum alloy, characterized in that: Using the aluminum alloy modifier according to any one of claims 1 to 5 comprises the following steps: S1. Add silicon-aluminum alloy raw materials into a melting furnace, heat to 860-920° C., keep warm for 15-30 minutes under an inert gas atmosphere, take samples for testing and adjust the composition to obtain silicon-aluminum alloy liquid; S2, at a temperature of 860-920° C., adding an aluminum alloy modifier to the silicon-aluminum alloy liquid obtained in step S1 at a ratio of 4-6% of the total weight of the silicon-aluminum alloy liquid, and stirring the mixture under an inert gas atmosphere for 10-15 minutes to obtain an alloy solution; S3, cooling the alloy solution obtained in step S2 to 740-760°C under stirring conditions at a cooling rate of 4-6°C / min under an inert gas atmosphere, and then keeping the mixture warm and stirring for 30-45min, and then keeping the mixture warm and standing for 15-20min to obtain a silicon-aluminum alloy liquid that has been subjected to a modification treatment; S4, casting the modified silicon-aluminum alloy liquid obtained in step S3.

7. The aluminum alloy modification method according to claim 6, characterized in that: In the step S1, the heating temperature is controlled at 880-900°C.

8. The aluminum alloy modification method according to claim 6, characterized in that: In the steps S1 to S3, the inert gas is argon.

9. The aluminum alloy modification method according to claim 6, characterized in that: In step S4, the casting temperature is controlled at 700-720°C, and the cooling rate is not less than 10 6 K / S.