Simplified preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties

By using graphene/natural rubber composite material with a dual crosslinking network structure in rubber tires, the problems of thermal aging and insufficient thermal conductivity of rubber tires are solved, and the effect of low heat generation and high thermal conductivity is achieved, and the service life of the tire is extended.

CN118006004BActive Publication Date: 2024-11-08ZHONGBEI UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410138941.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-01
Publication Date
2024-11-08
Estimated Expiration
2044-02-01

AI Technical Summary

Technical Problem

During the use of rubber tires, a large amount of heat is generated due to friction, which leads to heat generation problems. It is difficult for the prior art to effectively reduce the accumulation of heat inside the tire and improve thermal conductivity.

Method used

The simplified preparation process of graphene/natural rubber with low thermal generation and high thermal conductivity is adopted. Through the combination of graphene oxide and natural rubber, the thiol modification of thiol modified SiO2 with surface loaded in situ is formed. The dual crosslinking network structure of graphene oxide and natural rubber improves the interface interaction between filler-matrix and filler-fillers, and reduces frictional heat generation.

Benefits of technology

Effectively slow down the thermal aging speed of rubber tires, extend service life, improve the mechanical and thermal conductivity of the tires, reduce the frictional heat generation between the filler-matrix and the filler-filler, and achieve excellent performance with low heat generation and high heat conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118006004B_ABST
    Figure CN118006004B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of graphene and functional natural rubber composite materials, and in particular to a streamlined preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties. A thiol-modified graphene oxide aqueous dispersion with thiol-modified SiO2 grown on the surface load in situ is prepared by a simple and easily industrialized process. On the one hand, the dispersibility of graphene oxide in the rubber matrix can be improved, and on the other hand, the network structure constructed by the vulcanization process can improve the mechanical and thermal conductivity of the prepared natural rubber composite material, and the friction heat generation between the filler-matrix and the filler-filler is reduced. In addition, the modified graphene / natural rubber masterbatch is prepared by an efficient, energy-saving and easy-to-continuously produced water-phase synergistic coagulation process, which can not only reduce the number of mixing stages in the rubber preparation process, but also facilitate continuous mixing, shorten mixing time, reduce mixing energy consumption, reduce dust pollution, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene and functional natural rubber composite materials, and in particular to a streamlined preparation process of double-crosslinked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties. Background Art

[0002] Natural rubber (NR) has excellent properties such as high elasticity, high strength, high insulation, wear resistance and tear resistance. As a strategic resource, it plays an important role that cannot be replaced by artificial synthetic rubber. It is widely used in daily life and military fields, such as aircraft tires, engineering vehicle tires, and large-scale defense truck tires.

[0003] However, NR has no use strength, and only reinforced NR can be used in various products. In addition, the research on rubber toughening has a long history, and the main idea is to build a dissipative system in the elastic network. Based on this idea, many strategies have been developed in the reinforcement and toughening of NR, such as the introduction of nanocomposite structures, multiple crosslinking, copolymerization, metal coordination interactions, ionic interactions, and double network structures.

[0004] During driving, tires are affected by different stresses. While alternating external forces cause complex deformations, part of the energy is converted into heat energy due to the internal friction of the rubber, causing a large amount of heat to be generated inside the tire, which in turn causes temperature rise. The heat generation of rubber tires is mainly caused by the friction between fillers, fillers and rubber, and rubber and rubber. Therefore, it is necessary to reduce the heat accumulation inside the tire from two aspects: reducing the internal heat generation of NR composite materials and improving thermal conductivity. Improving the dispersibility of fillers in the matrix and enhancing the interactions between fillers, matrix and fillers can reduce the friction between fillers and fillers and between fillers and matrix, and improve the thermal conductivity of rubber. Therefore, improving the interface interactions between fillers, matrix and fillers is the key to achieving low heat generation and high thermal conductivity of rubber tires.

[0005] Graphene oxide has sp 2 The two-dimensional lamellar structure formed by the dense stacking of hybrid carbon atoms has the advantages of high thermal conductivity, high strength, good thermal stability, and large specific surface area. The large number of oxygen-containing functional groups on the surface provide active sites for modification of organic compounds.

[0006] Among the many technologies for preparing NR masterbatch, the emulsion blending method has significant advantages, such as being able to reduce the number of mixing stages in the preparation process, which is conducive to achieving continuous mixing, shortening mixing time, reducing mixing energy consumption, and reducing dust pollution. In addition, this method can also effectively improve the dispersion of fillers in the rubber matrix and the interfacial interaction between the two, and the shorter mixing time is also conducive to maintaining the molecular weight of NR, thereby ensuring the various properties of rubber composite materials. Summary of the invention

[0007] In order to slow down the thermal aging speed of rubber tires and prolong the service life, the present invention provides a simplified preparation process of double-crosslinked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties.

[0008] The present invention is achieved through the following technical solution: a simplified preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties, comprising the following steps:

[0009] (1) adding an activator and a catalyst to a graphene oxide aqueous dispersion under ice-water bath conditions, and after ultrasonic dispersion for a certain period of time, adding a silane coupling agent containing an amino group and a thiol group dissolved in an alkaline aqueous solution to the graphene oxide aqueous dispersion, so that the amino group of the silane coupling agent reacts with the carboxyl group on the surface of the graphene oxide to undergo an amidation reaction, and after a certain period of time, a thiol-modified graphene oxide aqueous dispersion is obtained;

[0010] (2) adding the aqueous dispersion of thiol-modified graphene oxide obtained in step (1) to an alcohol aqueous solution, adding a silicon source compound and a thiol-containing silane coupling agent at room temperature, reacting for a certain period of time to obtain thiol-modified graphene oxide particles with thiol-modified SiO2 grown in situ on the surface, washing with anhydrous ethanol and water, filtering until the filtrate is neutral, and preparing a uniform aqueous dispersion of thiol-modified graphene oxide with thiol-modified SiO2 grown in situ on the surface at a certain concentration;

[0011] (3) adding the uniform aqueous dispersion of thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface obtained in step (2) to natural rubber latex, stirring and mixing thoroughly to obtain a uniformly dispersed mixed emulsion, wherein the thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface forms bound particles with the rubber particles due to the electrostatic attraction of positive ions of the protein-phospholipid membrane on the surface of the rubber particles and remains stable; adding a flocculant, flocculation occurs because the repulsion between the particles that keeps the emulsion stable is reduced, and the bound particles and rubber particles are orderly aggregated in the aqueous phase and precipitated out in coordination; washing, dehydrating and drying the obtained raw rubber to obtain thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface / natural rubber masterbatch;

[0012] (4) adding the thiol-modified graphene oxide / natural rubber masterbatch with the surface loaded with in-situ grown thiol-modified SiO2 prepared in step (3) into an internal mixer, mixing at a certain temperature, adding rubber additives and reinforcing fillers in sequence, discharging the rubber material after uniform dispersion, and cooling to room temperature; then, mixing the rubber material on an open mixer at a certain temperature, adding a vulcanizing agent, mixing evenly, and thinning the rubber material until there are no bubbles in the rubber material, leaving it for a certain period of time, and then vulcanizing it at a certain temperature and a certain pressure for a certain period of time, so that the natural rubber reacts with the vulcanizing agent to form a vulcanized cross-linked network structure, and at the same time, the thiol-modified graphene oxide loaded with the in-situ grown thiol-modified SiO2 undergoes a vulcanization reaction with the rubber through the thiol end groups to form a double cross-linked network structure, thereby obtaining a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties.

[0013] As a further improvement of the technical solution of the present invention, in step (1), the temperature of the ice water bath is 0-4°C; the activator is selected from at least one of dicyclohexylcarbodiimide, diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride; the catalyst is selected from at least one of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, and N-hydroxysuccinimide; the mass of the graphene oxide in the graphene oxide aqueous dispersion is 0.1% by weight of the activator and the catalyst. The ratio is 1:0.01:0.01; the power of ultrasonic dispersion is 150-250W, and the time is 15-25min; the silane coupling agent containing both amino group and mercapto group is selected from at least one of 3-amino-4-mercaptopyridine, mercaptoethylamine, and 3-amino-5-mercapto-1,2,4-triazole, and the added amount of the silane coupling agent containing both amino group and mercapto group is 100-300% of the mass of graphene oxide in the graphene oxide aqueous dispersion; the time of amidation reaction is 8-16h.

[0014] As a further improvement of the technical solution of the present invention, in step (2), the volume ratio of ethanol to water in the alcohol-water solution is 5 to 9:1; the mercapto-containing silane coupling agent is selected from at least one of γ-thiopropyltriethoxysilane, (3-mercaptopropyl)trimethoxysilane, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide; the silicon source compound is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, and tetrapropyl orthosilicate; the mass ratio of the silicon source compound to graphene oxide is 30 to 90:1, and the mass ratio of the mercapto-containing silane coupling agent to graphene oxide is 2 to 4:3; and the reaction time after adding the silicon source compound and the mercapto-containing silane coupling agent is 5 to 9 hours.

[0015] As a further improvement of the technical solution of the present invention, in step (3), in the uniformly dispersed mixed emulsion, the mass ratio of the thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface to the natural rubber is 0.25 to 2.5:100; and the flocculant is selected from at least one of calcium chloride solution, sodium chloride solution, hydrochloric acid solution and formic acid solution.

[0016] As a further improvement of the technical solution of the present invention, in step (4), the surface of the mercapto-modified graphene oxide / natural rubber masterbatch loaded with in-situ grown mercapto-modified SiO2 comprises 100 parts by mass of natural rubber, 30 to 90 parts by mass of reinforcing filler, and 10 to 20 parts by mass of rubber additives.

[0017] As a further improvement of the technical solution of the present invention, in step (4), the rubber additives include an antioxidant, an antioxidant, an activator, a softener, and a vulcanization accelerator, and the mass ratio of the antioxidant, antioxidant, activator, softener, vulcanization accelerator and vulcanizer is 2:2:5:2:2:2.

[0018] As a further improvement of the technical solution of the present invention, in step (4), the reinforcing filler is carbon black, selected from at least one of models N110, N330 and N660.

[0019] As a further improvement of the technical solution of the present invention, in step (4), the mixing temperature of the mercapto-modified graphene oxide / natural rubber masterbatch with in-situ grown mercapto-modified SiO2 on the surface is 105-120°C in an internal mixer, and the mixing time is 12-20 min; the mixing temperature in an open mixer is 50-70°C, and the mixing time is 8-12 min.

[0020] As a further improvement of the technical solution of the present invention, in step (4), the storage time of the mixed rubber is 18 to 36 hours; the vulcanization temperature is 135 to 170° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 3 to 25 minutes.

[0021] The simplified preparation process of the double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties provided by the present invention has the following advantages compared with the prior art:

[0022] (1) A thiol-modified graphene oxide aqueous dispersion with in-situ grown thiol-modified SiO2 on the surface is prepared by a simple and easily industrialized process. On the one hand, the dispersibility of graphene oxide in the rubber matrix can be further improved. On the other hand, when the rubber composite material is vulcanized at a certain temperature and a certain pressure, the NR molecular chain undergoes a vulcanization cross-linking reaction with the vulcanizing agent to form a cross-linked network structure, while the thiol end groups of the thiol-modified SiO2 and the thiol-modified graphene react with the rubber molecular chain to form a single sulfur bond, which not only shortens the time required for the vulcanization of natural rubber and improves the processing performance, but also improves the interface interaction between graphene and the natural rubber matrix. The constructed double network structure improves the mechanical and thermal conductivity of the natural rubber composite material, reduces the frictional heat generated between the filler-matrix and the filler-filler, and obtains a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties.

[0023] (2) Using modified graphene oxide aqueous dispersion and natural rubber latex as raw materials, the modified graphene / natural rubber masterbatch is prepared by an efficient, energy-saving and easy-to-continuously produced aqueous phase synergistic coagulation process, which can not only reduce the number of mixing stages in the rubber preparation process, but also facilitate continuous mixing, shorten mixing time, reduce mixing energy consumption, reduce dust pollution, etc. The shorter mixing time is also conducive to maintaining the molecular weight of the rubber matrix, thereby ensuring the various properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 The infrared spectrum of the thiol-modified graphene oxide (characterized as SiO2-SH@GO-SH) with thiol-modified SiO2 grown in situ on the surface prepared in Example 1;

[0027] Figure 2 XRD spectrum of SiO2-SH@GO-SH prepared in Example 1;

[0028] Figure 3 This is the XPS spectrum of SiO2-SH@GO-SH prepared in Example 1;

[0029] Figure 4SEM photos of cross-sections of vulcanized rubbers of (a) the double-crosslinked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties prepared in Example 1, (b) the graphene oxide / natural rubber (GO / NR) prepared in Comparative Example 1, (c) the graphene oxide / natural rubber with in situ growth of SiO2 on the surface (SiO2@GO / NR) prepared in Comparative Example 3, and (d) the graphene oxide / natural rubber with in situ growth of thiol-modified SiO2 on the surface (SiO2-SH@GO / NR) prepared in Comparative Example 4.

[0030] The test method of the above-mentioned figure is:

[0031] Fourier transform infrared spectroscopy (FT-IR): The IS50 Fourier transform infrared spectrometer from Thermo Fisher Scientific was used to measure the sample in the transmission mode using the KBr pellet method. The spectral range was from 4000 to 500 cm -1 , resolution 8cm -1 Each sample was scanned 16 times. The spectra were baseline corrected using OMNIC software.

[0032] X-ray diffraction analysis (XRD): using Cu target material, Kα rays (λ=0.1546 nm) were continuously scanned on the sample to be tested, the scanning speed was 5° / min, and the scanning range was 5-80°.

[0033] X-ray photoelectron spectroscopy (XPS): The analysis was performed using the NEXSA X-ray photoelectron spectrometer from Thermo Fisher Scientific, USA. The CAE scanning mode was adopted, with a full spectrum scan energy of 160 eV and a narrow spectrum scan energy of 40 eV.

[0034] Field emission scanning electron microscope (SEM): The test was conducted using a Hitachi SU8010 scanning electron microscope at an accelerating voltage of 15KV. The rubber composite material was frozen with liquid nitrogen and immediately fractured, and the fracture surface was sprayed with conductive glue before testing.

[0035] Depend on Figure 1 It can be seen that the FT-IR spectrum of GO shows that hydroxyl (OH, 3433 cm -1 ), carbonyl or carboxyl (C=O, 1726cm -1 ), aromatic ring (C=C, 1619cm -1 ) and epoxy (CO, 1068cm -1 ) characteristic peak. Compared with GO, the spectrum of SiO2-SH@GO-SH has a peak at 1635cm -1 There is an obvious characteristic peak at 1083cm, which is the stretching vibration peak of O=CN, indicating that 3-amino-5-mercapto-1,2,4-triazole and GO undergo an amidation reaction; the characteristic peaks of carbonyl and epoxy groups disappear or weaken, and the peaks at 1083cm -1A new characteristic peak (Si-OC) merged with Si-O-Si appeared at 795 cm -1 A CS bond was generated at the site, indicating that GO underwent a dehydration condensation reaction with the silicon source compound and the silane coupling agent KH 580, indicating that SiO2-SH@GO-SH was successfully prepared.

[0036] Depend on Figure 2 It can be seen that: compared with GO, the characteristic peak of SiO2-SH@GO-SH at 10.91° disappears, and only one characteristic peak appears at 22.25°. According to the Bragg equation, the surface-loaded thiol-modified GO with in-situ grown thiol-modified SiO2 has a smaller interplanar spacing, indicating that GO is successfully modified.

[0037] Depend on Figure 3 It can be seen that: the XPS full spectrum shows that the surface of SiO2-SH@GO-SH contains N, S, and Si elements. The C 1s spectrum shows that the peak of O=CN appears at 289.28eV and the peak of CN appears at 286.08eV, indicating that 3-amino-5-mercapto-1,2,4-triazole undergoes an amidation reaction with GO; the Si-OC bond (102.78eV) appears in the Si 2p spectrum, and the CS bond (164.48eV) and -SH (163.28eV) appear in the S2p spectrum, indicating that the silicon source compound and the silane coupling agent KH 580 are successfully grafted onto GO, that is, SiO2-SH@GO-SH is successfully prepared.

[0038] Depend on Figure 4 It can be seen that SiO2-SH@GO-SH has the smallest flake size in NR vulcanizate and has the best dispersibility in the NR matrix. DETAILED DESCRIPTION

[0039] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0040] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0041] The present invention provides a specific embodiment of a simplified preparation process of a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties, comprising the following steps:

[0042] (1) adding an activator and a catalyst to a graphene oxide aqueous dispersion under ice-water bath conditions, and after ultrasonic dispersion for a certain period of time, adding a silane coupling agent containing an amino group and a thiol group dissolved in an alkaline aqueous solution to the graphene oxide aqueous dispersion, so that the amino group of the silane coupling agent reacts with the carboxyl group on the surface of the graphene oxide to undergo an amidation reaction, and after a certain period of time, a thiol-modified graphene oxide aqueous dispersion is obtained;

[0043] (2) adding the aqueous dispersion of thiol-modified graphene oxide obtained in step (1) to an alcohol aqueous solution, adding a silicon source compound and a thiol-containing silane coupling agent at room temperature, reacting for a certain period of time to obtain thiol-modified graphene oxide particles with thiol-modified SiO2 grown in situ on the surface, washing with anhydrous ethanol and water, filtering until the filtrate is neutral, and preparing a uniform aqueous dispersion of thiol-modified graphene oxide with thiol-modified SiO2 grown in situ on the surface at a certain concentration;

[0044] (3) adding the uniform aqueous dispersion of thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface obtained in step (2) to natural rubber latex, stirring and mixing thoroughly to obtain a uniformly dispersed mixed emulsion, wherein the thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface forms bound particles with the rubber particles due to the electrostatic attraction of positive ions of the protein-phospholipid membrane on the surface of the rubber particles and remains stable; adding a flocculant, flocculation occurs because the repulsion between the particles that keeps the emulsion stable is reduced, and the bound particles and rubber particles are orderly aggregated in the aqueous phase and precipitated out in coordination; washing, dehydrating and drying the obtained raw rubber to obtain thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface / natural rubber masterbatch;

[0045] (4) adding the thiol-modified graphene oxide / natural rubber masterbatch with the surface loaded with in-situ grown thiol-modified SiO2 prepared in step (3) into an internal mixer, mixing at a certain temperature, adding rubber additives and reinforcing fillers in sequence, discharging the rubber after uniform dispersion, and cooling to room temperature; then mixing the rubber on an open mixer at a certain temperature, adding a vulcanizing agent, mixing evenly, and thinning the rubber until there are no bubbles in the rubber, leaving it for a certain period of time, and then vulcanizing it at a certain temperature and a certain pressure for a certain period of time. In this process, on the one hand, the natural rubber and the vulcanizing agent undergo a vulcanization crosslinking reaction to form On the other hand, the thiol end groups of thiol-modified SiO2 and thiol-modified graphene react with the rubber molecular chains to form single sulfur bonds, which not only shortens the time required for the vulcanization of natural rubber and improves the processing performance, but also enhances the interfacial interaction between graphene and the natural rubber matrix. The constructed double network structure improves the mechanical and thermal conductivity of the final prepared natural rubber composite material, reduces the frictional heat generated between filler-matrix and filler-filler, and obtains a double-crosslinked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties.

[0046] The mechanism of preparing the thiol-modified graphene oxide with thiol-modified SiO2 grown in situ on the surface of the present invention is:

[0047]

[0048]

[0049] Taking the activator 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and the catalyst N-hydroxysuccinimide as an example, under the combined action of the activator and the catalyst, the carboxyl functional groups (-COOH) on the edge or surface of graphene oxide are activated, and undergo an amidation reaction with the amino groups (-NH2) on the amino- and mercapto-containing silane coupling agent (3-amino-5-mercapto-1,2,4-triazole). Subsequently, the added silicon source compound (tetrapropyl orthosilicate) and the mercapto-containing silane coupling agent (γ-mercaptopropyl triethoxysilane coupling agent; KH580) are first hydrolyzed in an alcohol aqueous solution, and then undergo a dehydration condensation reaction with the hydroxyl groups on the surface of graphene oxide, and finally a mercapto-modified graphene oxide with in-situ grown mercapto-modified SiO2 on the surface is obtained.

[0050] The mechanism of the formation of the dual cross-linked network structure in natural rubber composites is as follows:

[0051] ① The thiol-modified SiO2 in the thiol-modified graphene oxide with in-situ growth of thiol-modified SiO2 on the surface and the thiol end groups of thiol-modified graphene oxide respectively construct a cross-linked network connected by chemical bonds with the NR molecular chains. The relevant mechanism is:

[0052]

[0053] During the vulcanization process, -SH generates free radicals (-S·) and attacks the carbon-carbon double bonds of NR, triggering a series of polymerization reactions, resulting in cross-linking of NR.

[0054] ②NR reacts with the vulcanizing agent to form a vulcanized cross-linked network structure.

[0055] In one embodiment provided by the present invention, in step (1), the temperature of the ice water bath is 0-4°C; the activator is selected from at least one of dicyclohexylcarbodiimide, diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride; the catalyst is selected from at least one of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, and N-hydroxysuccinimide; the mass ratio of graphene oxide: activator: catalyst in the graphene oxide aqueous dispersion is The ratio of the silane coupling agent to the graphene oxide is 1:0.01:0.01; the power of the ultrasonic dispersion is 150 to 250 W, and the time is 15 to 25 min; the silane coupling agent containing both an amino group and a mercapto group is selected from at least one of 3-amino-4-mercaptopyridine, mercaptoethylamine, and 3-amino-5-mercapto-1,2,4-triazole, and the amount of the silane coupling agent containing both an amino group and a mercapto group added is 100 to 300% of the mass of the graphene oxide in the graphene oxide aqueous dispersion; and the time of the amidation reaction is 8 to 16 h.

[0056] In another embodiment provided by the present invention, in step (2), the volume ratio of ethanol to water in the alcohol-water solution is 5 to 9:1; the mercapto-containing silane coupling agent is selected from at least one of γ-thiopropyltriethoxysilane, (3-mercaptopropyl)trimethoxysilane, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide; the silicon source compound is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, and tetrapropyl orthosilicate; the mass ratio of the silicon source compound to graphene oxide is 30 to 90:1, and the mass ratio of the mercapto-containing silane coupling agent to graphene oxide is 2 to 4:3; and the reaction time after adding the silicon source compound and the mercapto-containing silane coupling agent is 5 to 9 hours.

[0057] In one embodiment provided by the present invention, in step (3), in the uniformly dispersed mixed emulsion, the mass ratio of the thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface to the natural rubber is 0.25 to 2.5:100; and the flocculant is selected from at least one of calcium chloride solution, sodium chloride solution, hydrochloric acid solution and formic acid solution.

[0058] In another embodiment provided by the present invention, in step (4), the surface of the mercapto-modified graphene oxide / natural rubber masterbatch loaded with in-situ grown mercapto-modified SiO2 comprises 100 parts by mass of natural rubber, 30 to 90 parts by mass of reinforcing filler, and 10 to 20 parts by mass of rubber additives.

[0059] In one embodiment provided by the present invention, in step (4), the rubber additives include an antioxidant, an antioxidant, an activator, a softener, and a vulcanization accelerator, and the mass ratio of the antioxidant, antioxidant, activator, softener, vulcanization accelerator and vulcanizer is 2:2:5:2:2:2.

[0060] In another embodiment provided by the present invention, in step (4), the reinforcing filler is carbon black, selected from at least one of models N110, N330 and N660.

[0061] In one embodiment provided by the present invention, in step (4), the mixing temperature of the mercapto-modified graphene oxide / natural rubber masterbatch with in-situ grown mercapto-modified SiO2 on the surface in an internal mixer is 105-120°C, and the mixing time is 12-20 min; the mixing temperature in an open mixer is 50-70°C, and the mixing time is 8-12 min.

[0062] In another embodiment provided by the present invention, in step (4), the storage time of the rubber mix is ​​18 to 36 hours; the vulcanization temperature is 135 to 170° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 3 to 25 minutes.

[0063] The specific embodiments of the present invention are described in detail below.

[0064] Example 1

[0065] A simplified preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties, comprising the following steps:

[0066] (1) Add 0.0015 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) and 0.0015 g of N-hydroxysuccinimide (NHS) to a container containing 30 g of 0.5 wt.% GO aqueous dispersion placed in an ice-water bath at 0°C, and ultrasonicate for 20 min at 200 W. Add 0.3 g of 3-amino-5-mercapto-1,2,4-triazole powder to 50 g of deionized water, and add 5% sodium hydroxide to adjust the pH value to 13. After all the water is dissolved, add it to the ultrasonicated GO aqueous dispersion and react for 12 h to obtain a thiol-modified GO aqueous dispersion.

[0067] (2) At room temperature, 120 mL of an alcohol-water solution was prepared in a mass ratio of ethanol to water of 7:1, and then the thiol-modified GO aqueous dispersion obtained in step (1) was added, followed by the addition of 9 mL of tetrapropyl orthosilicate (TPOS) and 0.15 mL of γ-thiopropyltriethoxysilane (KH580). The mixture was reacted at room temperature for 9 h to obtain thiol-modified graphene oxide particles (SiO2-SH@GO-SH) with in situ grown thiol-modified SiO2 on the surface. The particles were washed with anhydrous ethanol and water, filtered until the filtrate was neutral, and then a uniform aqueous dispersion of SiO2-SH@GO-SH with a concentration of 5 mg / mL was prepared.

[0068] (3) adding the SiO2-SH@GO-SH uniform aqueous dispersion containing 0.5 g SiO2-SH@GO-SH obtained in step (2) to 333.4 g 30 wt.% natural rubber latex, stirring and mixing thoroughly to obtain a uniformly dispersed mixed emulsion; adding a flocculant calcium chloride solution to demulsify and flocculate the mixed emulsion; washing the flocculent blocks with water, dehydrating, and drying at 60° C. to constant weight to obtain a thiol-modified graphene oxide / natural rubber masterbatch with in-situ grown thiol-modified SiO2 on the surface;

[0069] (4) Add the thiol-modified graphene oxide / natural rubber masterbatch containing 100g of natural rubber surface-loaded in-situ grown thiol-modified SiO2 prepared in step (3) into an internal mixer and mix at 110°C for 4min; then add 2g of antioxidant 2,2,4-trimethyl-1,2-dihydroquinoline polymer, 2g of antioxidant N-(1-methylisopentyl)-N'-phenyl-p-phenylenediamine, and 2g of vulcanization accelerator N-(oxydiethylene)-2-benzothiazolesulfonamide in sequence, mix for 4min, and then add 5g of activator zinc oxide, 2g of softener stearic acid in sequence. , 30g of N330 carbon black, kneading for 4min; then add 30g of N330 carbon black, kneading for 4min and then discharge the rubber; after the rubber is cooled to room temperature, transfer it to an open mixing mill for kneading at 60℃, add 2g of sulfur during the kneading process, mix evenly after kneading for 8min, and then pass it through a thin tube until there are no bubbles in the rubber. After standing for 24h, place it in a vulcanization mold, and vulcanize Tc90 (5min; tested by RPA rubber processing analyzer) at 150℃ and 15MPa to obtain a double-crosslinked network graphene / natural rubber vulcanizate with low heat generation, high thermal conductivity and excellent mechanical properties.

[0070] Example 2

[0071] A simplified preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties, comprising the following steps:

[0072] The process is exactly the same as that of Example 1, except that the amount of 3-amino-5-mercapto-1,2,4-triazole powder added in step (1) is 0.15 g.

[0073] Example 3

[0074] A simplified preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties, comprising the following steps:

[0075] The process is exactly the same as that of Example 1, except that the amount of 3-amino-5-mercapto-1,2,4-triazole powder added in step (1) is 0.45 g.

[0076] Comparative Example 1:

[0077] A method for preparing a graphene oxide / natural rubber composite material comprises the following steps:

[0078] (1) 50 g of 1 wt.% GO aqueous dispersion was mixed with 50 g of deionized water and ultrasonicated at 200 W for 20 min to prepare a 5 mg / mL GO dispersion.

[0079] (2) The same as step (3) of Example 1, except that the GO aqueous dispersion prepared in step (1) is added to the natural rubber latex.

[0080] (3) The same as step (4) of Example 1 was used to prepare GO / NR vulcanized rubber.

[0081] Comparative Example 2:

[0082] A method for preparing a thiol-modified graphene oxide / natural rubber composite material comprises the following steps:

[0083] (1) Same as step (1) of Example 1.

[0084] (2) The same as step (3) of Example 1, except that the aqueous dispersion of mercapto-modified GO (GO-SH) prepared in step (1) is added to the natural rubber latex.

[0085] (3) The same as step (4) of Example 1 was used to prepare GO-SH / NR vulcanized rubber.

[0086] Comparative Example 3:

[0087] A simplified preparation process of graphene oxide / natural rubber with in-situ growth of SiO2 on the surface, comprising the following steps:

[0088] (1) 120 mL of alcohol-water solution was prepared at room temperature in a mass ratio of ethanol to water of 7:1, and then 15 g of 1 wt.% GO aqueous dispersion was added. The mixture was ultrasonicated at 200 W for 20 min, and then 9 mL of tetrapropyl orthosilicate (TPOS) was added and the pH was adjusted to 13 by adding 5% sodium hydroxide. The mixture was reacted at room temperature for 9 h to obtain graphene oxide particles with in situ grown SiO2 on the surface (SiO2@GO). The particles were washed with anhydrous ethanol and water, filtered until the filtrate was neutral, and then a uniform SiO2@GO aqueous dispersion with a concentration of 5 mg / mL was prepared.

[0089] (2) The same as step (3) of Example 1, except that the SiO2@GO aqueous dispersion prepared in step (1) is added to the natural rubber latex.

[0090] (3) The same as step (4) of Example 1 was used to prepare SiO2@GO / NR vulcanized rubber.

[0091] Comparative Example 4:

[0092] A simplified preparation process for graphene oxide / natural rubber with in-situ growth of mercapto-modified SiO2 on the surface, comprising the following steps:

[0093] (1) Same as step (2) of Example 1, except that GO dispersion is added.

[0094] (2) The same as step (3) of Example 1, except that the mercapto-modified SiO2-SH@GO aqueous dispersion prepared in step (1) is added to the natural rubber latex.

[0095] (3) The same as step (4) of Example 1 was used to prepare SiO2-SH@GO / NR vulcanized rubber.

[0096] Table 1 shows the properties of the rubber composite materials prepared in Examples 1-3 and Comparative Examples 1-4. The tensile performance test was conducted on an AI-7000 tensile machine of Taiwan High Speed ​​Rail Technology Co., Ltd., the test standard was ISO 37-2005, and the tensile rate was 500 mm / min. The test standard for tearing performance was GB / T 529-2008. The test standard for fatigue compression heat generation performance was GB / T 1687.1-2016. The test standard for thermal conductivity was GB / T11205-2009.

[0097] Table 1. Properties of the prepared rubber composites

[0098]

[0099]

[0100] As can be seen from Table 1, the low heat generation, high thermal conductivity, excellent mechanical properties double cross-linked network graphene / natural rubber prepared by the present invention has excellent mechanical properties and high thermal conductivity and low heat generation. This is due to the synergistic effect of thiol modification and in-situ grown SiO2, which makes the modified GO well dispersed in the NR matrix and also participates in the cross-linking of NR; and the double network structure constructed in the vulcanized rubber improves the mechanical and thermal conductivity of the prepared NR composite material, and reduces the frictional heat between the filler-matrix and the filler-filler; thus, the low heat generation, high thermal conductivity, excellent mechanical properties double cross-linked network graphene / natural rubber is obtained.

[0101] The above is only a specific implementation of the present invention, which enables those skilled in the art to understand or implement the present invention. Although detailed descriptions are given with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments, and they should all be covered by the protection scope of the claims.

Claims

1. A simplified preparation process of double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties, characterized in that it comprises the following steps: (1) Adding an activator and a catalyst to a graphene oxide aqueous dispersion under ice-water bath conditions, and after ultrasonic dispersion for 15 to 25 minutes, adding a silane coupling agent containing an amino group and a mercapto group dissolved in an alkaline aqueous solution to the graphene oxide aqueous dispersion, the amino group of the silane coupling agent reacts with the carboxyl group on the surface of the graphene oxide to undergo an amidation reaction, and after 8 to 16 hours, a mercapto-modified graphene oxide aqueous dispersion is obtained; (2) adding the aqueous dispersion of thiol-modified graphene oxide obtained in step (1) to an alcohol aqueous solution, adding a silicon source compound and a thiol-containing silane coupling agent at room temperature, reacting for 5 to 9 hours, obtaining thiol-modified graphene oxide particles with thiol-modified SiO2 grown in situ on the surface, washing with anhydrous ethanol and water, filtering until the filtrate is neutral, and preparing a uniform aqueous dispersion of thiol-modified graphene oxide with thiol-modified SiO2 grown in situ on the surface at a certain concentration; (3) adding the uniform aqueous dispersion of thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface obtained in step (2) to natural rubber latex, stirring and mixing thoroughly to obtain a uniformly dispersed mixed emulsion, wherein the thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface forms bound particles with the rubber particles due to the electrostatic attraction of positive ions of the protein-phospholipid membrane on the surface of the rubber particles and remains stable; adding a flocculant, flocculation occurs because the repulsion between the particles that keeps the emulsion stable is reduced, and the bound particles and rubber particles are orderly aggregated in the aqueous phase and precipitated out in coordination; washing, dehydrating and drying the obtained raw rubber, thereby obtaining thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface / natural rubber masterbatch; (4) The thiol-modified graphene oxide / natural rubber masterbatch with in-situ grown thiol-modified SiO2 on the surface prepared in step (3) is added to an internal mixer, and internally mixed at a certain temperature of 105-120°C. A rubber additive and a reinforcing filler are added in sequence, and the rubber is discharged after being evenly dispersed, and cooled to room temperature. The rubber is then open-mixed on an open mixer at a certain temperature of 50-70°C, a vulcanizing agent is added, and after being evenly mixed, the rubber is thinly passed until there are no bubbles in the rubber. After standing for 18-36 hours, the rubber is vulcanized at a vulcanization temperature of 135-170°C and a pressure of 10-30 MPa for 3-25 minutes, so that the natural rubber reacts with the vulcanizing agent to form a vulcanized cross-linked network structure, and at the same time, the thiol-modified graphene oxide loaded with in-situ grown thiol-modified SiO2 undergoes a vulcanization reaction with the rubber through the thiol end group to form a double cross-linked network structure, thereby obtaining a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties.

2. The simplified preparation process of a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1, characterized in that, in step (1), the temperature of the ice water bath is 0-4 ° C; the activator is selected from at least one of dicyclohexylcarbodiimide, diisopropylcarbodiimide, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride; the catalyst is selected from at least one of 4-N,N-dimethylpyridine, 1-hydroxybenzotriazole, and N-hydroxysuccinimide; the mass ratio of graphene oxide: activator: catalyst in the graphene oxide aqueous dispersion is 1:0.01:0.01; the power of ultrasonic dispersion is 150~250W; the silane coupling agent containing both amino and mercapto groups is selected from at least one of 3-amino-4-mercaptopyridine, mercaptoethylamine, and 3-amino-5-mercapto-1,2,4-triazole, and the amount of the silane coupling agent containing both amino and mercapto groups added is 100~300% of the mass of graphene oxide in the graphene oxide aqueous dispersion.

3. A streamlined preparation process for a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1, characterized in that, in step (2), the volume ratio of ethanol to water in the alcohol-water solution is 5-9:1; the mercapto-containing silane coupling agent is selected from at least one of γ-thiopropyltriethoxysilane, (3-mercaptopropyl)trimethoxysilane, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide; the silicon source compound is selected from at least one of tetramethyl orthosilicate, tetraethyl orthosilicate, and tetrapropyl orthosilicate; the mass ratio of the silicon source compound to graphene oxide is 30-90:1, and the mass ratio of the mercapto-containing silane coupling agent to graphene oxide is 2-4:

3.

4. The simplified preparation process of a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1 is characterized in that, in step (3), in the uniformly dispersed mixed emulsion, the mass ratio of the thiol-modified graphene oxide with in-situ grown thiol-modified SiO2 on the surface to the natural rubber is 0.25~2.5:100; and the flocculant is selected from at least one of calcium chloride solution, sodium chloride solution, hydrochloric acid solution and formic acid solution.

5. The streamlined preparation process of a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1, characterized in that, in step (4), the surface-loaded in-situ grown thiol-modified SiO2 in the thiol-modified oxide graphene / natural rubber masterbatch comprises 100 parts by mass of natural rubber, 30 to 90 parts by mass of reinforcing filler and 10 to 20 parts by mass of rubber additives.

6. The streamlined preparation process of a double-crosslinked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1, characterized in that, in step (4), the rubber additives include an antioxidant, an antioxidant, an activator, a softener, and a vulcanization accelerator, and the mass ratio of the antioxidant, antioxidant, activator, softener, vulcanization accelerator and vulcanizer is 2:2:5:2:2:

2.

7. The streamlined preparation process of a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1, characterized in that in step (4), the reinforcing filler is carbon black, selected from at least one of models N110, N330 and N660.

8. The streamlined preparation process of a double cross-linked network graphene / natural rubber with low heat generation, high thermal conductivity and excellent mechanical properties according to claim 1, characterized in that, in step (4), the thiol-modified graphene oxide / natural rubber masterbatch with in-situ grown thiol-modified SiO2 on the surface is mixed in an internal mixer for 12 to 20 minutes; and in an open mixer for 8 to 12 minutes.

Citation Information

Patent Citations

  • Preparation method for modified graphene oxide, MGO-SiO2 nano-hybrid material and MGO-SiO2 modified phenolic resin hot melting adhesive film

    CN106520040A

  • Hindered phenol functionalized graphene as well as preparation method and application thereof

    CN107857897A

  • Preparation method of graphene-silicon dioxide modified natural rubber composite material with high thermal conductivity, low thermodynamic property and excellent mechanical property for tires

    CN113462040A

  • Method of preparing graphene / natural rubber composite with enhanced mechanical properties, thermal conductivity, and wear resistance

    US11732112B1