Slurry for rare earth-based high band gap filler for radiant cooling coating and preparation method thereof
Through the preparation of slurry for rare earth-based high-bandgap fillers, the problems of unstable titanium dioxide quality and ultraviolet absorption are solved, high stability, full-band solar light reflection and high atmospheric window emissivity are achieved, and the performance of radiation refrigeration coatings is improved. .
Patent Information
- Application Number
- CN202410042688.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-01-11
AI Technical Summary
The rutile titanium dioxide products in existing radiation refrigeration coatings are unstable in quality and have strong absorption of ultraviolet rays, which affects the solar light reflection and heat dissipation performance of the coating.
Using rare earth-based high band gap filler slurry, by mixing materials such as tungsten oxide, niobium oxide and rare earth oxide, ball milling, sintering, amorphous powder with high band gap width is formed, combining particle size control and dispersant Used to prepare fillers with excellent sunlight reflection and atmospheric window emission properties.
It achieves high stability of fillers, low UV absorption, full-band solar light reflection effect and high atmospheric window emissivity, improving the performance and service life of radiation refrigeration coatings.
Smart Images

Figure CN118006155B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new material preparation, and particularly relates to a slurry for rare earth-based high band gap filler for radiant refrigeration coating and a preparation method thereof. Background Art
[0002] Radiative cooling coatings are a new type of coating product in recent years. This type of product is mainly used in outdoor environments, such as walls, clothing, car paint, etc. There are two core performance requirements. On the one hand, the coating is required to have excellent sunlight reflection performance, which can minimize the incidence of sunlight and reduce energy input. On the other hand, this type of coating is required to have excellent "atmospheric window" (8-13μm) emission performance, which can permanently discharge heat to the universe outside the atmosphere, thereby achieving excellent heat dissipation performance.
[0003] The realization of the core function of radiant cooling coatings depends on the filler in the coating. In the prior art, the most commonly used sunlight reflective filler is rutile titanium dioxide. However, this material has the following two problems in actual use:
[0004] 1. The quality of titanium dioxide products is unstable. As we all know, titanium dioxide has three crystal forms, namely rutile, anatase and brookite. The crystal form of titanium dioxide is affected by the production process and synthesis conditions. Therefore, in actual production, it is difficult to obtain rutile titanium dioxide with stable crystal quality and high purity at a low cost.
[0005] 2. Titanium dioxide will absorb ultraviolet rays in sunlight to a certain extent. The degree of solar reflectivity is one of the important core indicators of radiative cooling coatings. High solar reflectivity fillers require not only that the material has reflective properties for visible light and near-infrared rays in sunlight, but also that the material has excellent reflective properties for ultraviolet rays in sunlight. However, rutile titanium dioxide will absorb ultraviolet rays in sunlight to a certain extent, mainly because the band gap width (Eg) of the material is too low. The Eg of rutile titanium dioxide is about 2.8-2.9 eV. When exposed to sunlight, ground state electrons absorb ultraviolet rays and undergo transitions.
[0006] Titanium dioxide's absorption of ultraviolet rays will greatly affect the performance of radiation cooling coatings: on the one hand, the coating's absorption of ultraviolet rays will increase the energy input of sunlight and reduce the coating's cooling performance; on the other hand, after the filler absorbs ultraviolet rays, the excited electrons will destroy the molecular bonds of the resin material in the coating, accelerate the aging of the coating, and destroy the product performance.
[0007] In the prior art, titanium dioxide is often mixed with other low UV absorption materials (such as barium sulfate, silicon dioxide, glass beads, etc.) to reduce the absorption of UV by coatings. However, this method does not change the problem of too low band gap of titanium dioxide, and the reduction of its UV absorption performance is at the expense of the reflection effect. Summary of the invention
[0008] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a slurry for rare earth-based high bandgap fillers for radiant cooling coatings and a preparation method thereof, wherein the slurry has a relatively high bandgap width, reduces the absorption of ultraviolet rays by the filler, and simultaneously achieves the effects of high sunlight reflection and high atmospheric window emissivity.
[0009] The objective of the present invention is achieved through the following technical solutions:
[0010] A method for preparing a slurry for a rare earth-based high band gap filler for a radiative cooling coating comprises the following steps:
[0011] S1. In parts by weight, 20-35 parts of tungsten oxide, 25-36 parts of niobium oxide, 13-20 parts of rare earth oxides and 16-35 parts of boron oxide are fully mixed and then ball milled and powdered to obtain a precursor powder;
[0012] S2. The precursor powder is smelted and sintered to obtain a molten liquid;
[0013] S3. The molten liquid was poured into cold water and quenched, and after filtering and drying, a powder A was obtained;
[0014] S4. A liquid reagent was added to the powder A to prepare a mixed solution, and a dispersant was added to the mixed solution and then sand-milled to obtain slurries A1, A2, and A3 with different median particle sizes;
[0015] S5. The slurries A1, A2 and A3 are uniformly mixed to obtain a product slurry;
[0016] Wherein, the rare earth oxide includes cerium oxide or lanthanum oxide.
[0017] Furthermore, in step S1, the ball milling adopts a planetary ball mill, the rotation speed of the ball mill is 400r / min, the ratio of large, medium and small balls is 3:4:3, the volume ratio of air, liquid and balls in the ball milling chamber is 1:1:1, and the ball milling time is 12h.
[0018] Furthermore, in step S2, the smelting and sintering includes five stages, specifically:
[0019] In the first stage, the temperature was raised evenly from 50°C to 400°C, and the heating time was 35 minutes;
[0020] The second stage was kept at 400°C for 30 min;
[0021] In the third stage, the temperature is evenly increased from 400°C to 900°C, and the heating time is 60 minutes;
[0022] In the fourth stage, the temperature is evenly increased from 900°C to 1400°C, and the heating time is 120 min;
[0023] The fifth stage is kept at 1400°C for 240 minutes.
[0024] Furthermore, when the fifth stage is performed, after keeping the temperature for 180 minutes, the slurry is stirred at a speed of 60 r / min for 30 minutes, and then the temperature is kept until the sintering is completed.
[0025] Furthermore, in step S4, the liquid reagent includes water or butyl acetate, the content of the powder A in the mixed liquid is 40%, and the choice of solvent depends on the demand of the coating product. For water-based coating slurry, the solvent is water; for oil-based coating, the solvent is butyl acetate.
[0026] Furthermore, in step S4, the dispersant includes BYK111 type dispersant, and the added amount of the dispersant is 12-15% of the mass of the mixed liquid.
[0027] Furthermore, in step S4, the median particle size of the slurry A1 is 15-25 μm, the median particle size of the slurry A2 is 1-7 μm, and the median particle size of the slurry A3 is 0.3-0.7 μm.
[0028] Furthermore, in step S5, the mass ratio of the slurries A1, A2 and A3 is 1:0.8-1.3:0.4-0.6.
[0029] The present invention also provides a slurry for rare earth-based high band gap filler used in radiation refrigeration coating obtained by the above preparation method.
[0030] The present invention also provides application of the slurry in preparing radiation cooling coating.
[0031] The beneficial effects of the present invention are:
[0032] 1. High stability of product quality. The quality of titanium dioxide raw materials is unstable because there are various crystal structures, and the formation of these crystal structures is affected by various factors such as production process and production conditions. High-quality rutile titanium dioxide requires strict control of production process, but this also increases production costs. One of the innovations of the present invention is that amorphous oxide is used as raw material, and after the raw material is melted into a glass body, the molecules have an amorphous structure. Since there is no crystal structure, the stability of product quality can be fundamentally guaranteed.
[0033] 2. The filler powder has a higher band gap and lower ultraviolet absorption performance. In addition to the influence of the crystal form, the absorption of ultraviolet rays by titanium dioxide is also related to the intrinsic properties of the titanium element. Based on this, the present invention improves the band gap of the filler material and reduces its absorption of ultraviolet rays by selecting elements and adjusting the element content; element selection refers to the use of materials such as tungsten oxide and niobium oxide with higher band gaps to replace titanium oxide. Among them, the band gap of tungsten oxide is about 3.2 eV, and the band gap of niobium oxide is 3.4 eV. Using high band gap materials as raw materials can reduce the absorption of ultraviolet rays by the product filler. On the other hand, the band gap can be further adjusted by adjusting the element content, thereby fundamentally reducing the absorption of ultraviolet rays by the material. Compared with the crystalline materials in the prior art, due to their definite elemental composition and crystal structure, their band gaps are often deterministic, and the ultraviolet absorption performance cannot be adjusted by adjusting the content of different elements.
[0034] 3. In the production method, the particle size is specially controlled to obtain the highest reflection efficiency. When the filler reflects infrared rays, it essentially generates Mie scattering with the incident light, and the scattering intensity is related to the shape factor of the filler. Simply put, large-particle fillers have a better reflection effect on infrared rays with a longer wavelength, and small-particle filler particles have a better reflection effect on incident light with a shorter wavelength. In the prior art, the fillers used are often fillers with uniform particle sizes obtained by ball milling or sand milling. Such fillers only have a good reflection effect on incident light of a certain wavelength, and have a poor reflection effect on incident light of other wavelengths. When used as fillers for radiant cooling coatings, their reflection performance for the full band of sunlight is poor. In the production process of the present invention, through process control, the powder material is first processed into an intermediate raw material with a certain particle size, and then the powders of each particle size distribution are carefully proportioned according to a certain content, and finally a filler product with multiple particle size distributions is obtained, which can produce excellent reflection effects for sunlight of the full band.
[0035] 4. With radiation cooling coating as the application direction, the window emissivity of filler powder is improved by introducing rare earth elements. High atmospheric window emissivity is one of the core indicators of radiation cooling coating. The titanium dioxide filler commonly used in the prior art has a very low emissivity in the atmospheric window band. Therefore, when actually preparing radiation cooling coating, other high-emissivity fillers need to be added to achieve high window emissivity. Among the many high-emissivity fillers, rare earth materials, especially rare earth oxide materials represented by lanthanum cerium oxide materials, are ideal materials for high-emissivity materials because they have a high emissivity at 8-14 microns. However, rare earth oxide materials represented by cerium oxide are themselves a commonly used ultraviolet absorption material with excellent ultraviolet absorption performance. The mutual matching of titanium dioxide and lanthanum cerium rare earth oxide will reduce the sunlight reflection effect of the filler, which makes the filler face the problem of choosing between high infrared reflection and high window emissivity. The present invention uses the same material to achieve high sunlight reflection and high window emissivity at the same time, which fully meets the application requirements of radiation cooling coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The XRD test results of powder A in Example 1 are as follows;
[0037] Figure 2 The reflectivity test results of the slurry in Example 1 are as follows;
[0038] Figure 3 This is a graph showing the bandgap test results of the slurry of Example 1. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.
[0040] A method for preparing a slurry for a rare earth-based high band gap filler for a radiative cooling coating comprises the following steps:
[0041] S1. According to weight, weigh 20 parts of tungsten oxide, 26 parts of niobium oxide, 16 parts of cerium oxide, and 30 parts of boric acid, mix them thoroughly, add a certain amount of water, and wet grind them in a planetary ball mill. The speed of the ball mill is 400 r / min, the ratio of large, medium and small balls is 3:4:3, the volume ratio of air: liquid: ball in the cavity is controlled at 1:1:1, and the grinding time is 12 h; after grinding, filter the grinding beads with a 40-mesh screen to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in a 90°C oven to obtain a precursor sample that is agglomerated into a block. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder.
[0042] S2. The precursor powder is loaded into a corundum crucible and heated in a melting furnace with a stirring paddle, wherein the heating program is:
[0043] In the first stage, the temperature was raised evenly from 50°C to 400°C, and the heating time was 35 min;
[0044] The second stage was kept at 400°C for 30 min;
[0045] In the third stage, the temperature was raised evenly from 400°C to 900°C, and the heating time was 60 min;
[0046] In the fourth stage, the temperature was raised evenly from 900°C to 1400°C, and the heating time was 120 min;
[0047] The fifth stage is kept at 1400°C for 240 min.
[0048] After the fifth stage of heat preservation for 3 hours, the corundum stirring paddle was lowered into the liquid and slowly stirred at a speed of 60r / min for 30 minutes, and then the stirring paddle was lifted. After the heating program was completed, a molten liquid was obtained;
[0049] S3. The molten liquid was poured into cold water and quenched, filtered and dried to obtain a powder A;
[0050] S4. Add water to the powder A to prepare a mixed solution in which the content of powder A accounts for 40%, and add BYK111 type dispersant of about 14% by weight of the mixed solution, then put it into a sand mill for sand grinding, the grinding ball particle size is 0.3-0.5mm, and the slurry particle size is measured once every 15 minutes with a laser particle size analyzer, and slurry A1 with a median particle size (D50) of 19.5μm, slurry A2 with a D50 of 4.2μm, and slurry A3 with a D50 of 0.63μm are obtained respectively;
[0051] S5. Mix the slurry in a mass ratio of A1:A2:A3=1:1.02:0.5, and stir well with a stirring plate to obtain a finished slurry.
[0052] The XRD test results of powder A are as follows: Figure 1 As shown, it can be seen that within the scanning angle range, the intensity of the scattered X-rays changes smoothly without independent peaks, indicating that powder A is an amorphous material.
[0053] For the reflective performance, the slurry needs to be prepared into a coating sample for testing. The specific method is to take 30 g of water-based acrylic resin with a solid content of 35%, 60 g of finished slurry, add appropriate amount of water to adjust the viscosity of the coating, and evenly apply the coating on the surface of the aluminum sheet. After the resin is completely cured and dried, the reflective effect is tested with a UV-visible-infrared spectrophotometer. The results are as follows Figure 2 As shown, it has a good reflection effect (more than 90%) in the whole band.
[0054] The bandgap of the slurry was tested using a Lamba 1050 spectrum analyzer, and the results were calculated according to the following formula:
[0055] αhv = A(hv − Eopt) 2
[0056] Among them, α is the absorptivity, the sum of the absorptivity and the reflectivity of the incident light of this wavelength is equal to 1, and hv is the energy level of the incident light wavelength, in eV.
[0057] Figure 3 Graph showing the bandgap test results. The bandgap value is obtained by extrapolating the straight line portion to the intersection of the horizontal axis. It can be seen that the bandgap of the slurry of the present invention reaches 3.7 eV, which is higher than 2.7-2.8 eV of titanium dioxide. Therefore, the absorption of ultraviolet rays by the slurry of the present invention is much lower than that of titanium dioxide.
[0058] The emissivity of the slurry was tested using an IR-1 hemispherical emissivity tester. The test method was based on GB / T25261-2018 "Reflective Thermal Insulation Coatings for Buildings". At 25°C, the window emissivity at 8-14 μm was measured to be 0.96, demonstrating excellent emissivity performance.
[0059] A method for preparing a slurry for a rare earth-based high band gap filler for a radiative cooling coating comprises the following steps:
[0060] S1. According to weight, weigh 30 parts of tungsten oxide, 35 parts of niobium oxide, 16 parts of lanthanum oxide, and 16 parts of boric acid, mix them thoroughly, add a certain amount of water, and wet grind them in a planetary ball mill. The speed of the ball mill is 400 r / min, the ratio of large, medium and small balls is 3:4:3, the volume ratio of air: liquid: ball in the cavity is controlled at 1:1:1, and the grinding time is 12 h; after grinding, filter the grinding beads with a 40-mesh screen to obtain a coarsely ground slurry. The coarsely ground slurry is fully dried in a 90°C oven to obtain a precursor sample that is agglomerated into a block. The block precursor sample is put into a powder crusher again to obtain a uniformly mixed precursor powder.
[0061] S2. The powder is loaded into a corundum crucible and heated in a melting furnace with a stirring paddle, wherein the heating program is: in the first stage, the temperature is evenly increased from 50°C to 400°C, and the heating time is 35min;
[0062] The second stage was kept at 400°C for 30 min;
[0063] In the third stage, the temperature was raised evenly from 400°C to 900°C, and the heating time was 60 min;
[0064] In the fourth stage, the temperature was raised evenly from 900°C to 1400°C, and the heating time was 120 min;
[0065] The fifth stage is kept at 1400°C for 240 min.
[0066] After the fifth stage of heat preservation for 3 hours, the corundum stirring paddle was lowered into the liquid and slowly stirred at a speed of 60 revolutions per minute for 30 minutes, and then the stirring paddle was lifted. After the heating program was completed, a molten liquid was obtained;
[0067] S3. The molten liquid was poured into cold water and quenched, filtered and dried to obtain a powder A;
[0068] S4. Add butyl acetate to the powder A to prepare a mixed solution in which the content of powder A accounts for 40%, and add 15% of the weight of the mixed solution BYK111 type dispersant, and then put it into a sand mill for sand grinding. The grinding ball particle size is 0.3-0.5mm. The slurry particle size is measured once every 15 minutes using a laser particle size analyzer to obtain slurry A1 with a D50 of 19.5μm, slurry A2 with a D50 of 4.2μm, and slurry A3 with a D50 of 0.63μm;
[0069] S5. Mix the slurry in a mass ratio of A1:A2:A3=1:1.12:0.5, and stir well with a stirring plate to obtain a finished slurry.
[0070] Comparative Example 1
[0071] The difference between Comparative Example 1 and Example 1 is that the particle size of the finished slurry is uniform. That is, in step S4, the powder A is uniformly sand-ground to a finished slurry with a D50 of 20 μm, and the remaining steps are the same.
[0072] Comparative Example 2
[0073] The difference between Comparative Example 2 and Example 1 is that the rare earth oxide cerium oxide is not added to the components of the slurry, and the other steps are the same.
[0074] Comparative Example 3
[0075] In Comparative Example 3, rutile titanium dioxide with a median particle size of 5-6 μm purchased from Shanghai Yuejiang was used as the slurry.
[0076] The slurries of Example 2 and Comparative Examples 1-3 were tested for solar reflectivity and atmospheric window emissivity in the same manner. The test results are shown in Table 1 (average values):
[0077] Table 1
[0078] Solar reflectivity (%) Atmospheric window emissivity Example 2 91.3 0.96 Comparative Example 1 85.2 0.95 Comparative Example 2 86.5 0.91 Comparative Example 3 90.2 0.55
[0079] Slurry stability test:
[0080] The molten liquid obtained after steps S1 and S2 in Example 1 is poured onto the surface of a horizontally placed stainless steel plate while hot, and is allowed to cool naturally in the air to obtain a solid.
[0081] Comparative Example 4
[0082] 40 parts of tungsten oxide, 15 parts of niobium oxide, 30 parts of cerium oxide and 7 parts of boric acid were weighed by weight, and steps S1 and S2 in Example 1 were carried out. The obtained molten liquid was poured onto the surface of a horizontally placed stainless steel plate while hot, and allowed to cool naturally in the air.
[0083] The difference between Comparative Example 4 and Example 3 is that the ratios of the raw materials used to prepare the slurry are different.
[0084] Comparative Example 5
[0085] 15 parts of tungsten oxide, 26 parts of niobium oxide, 10 parts of cerium oxide and 40 parts of boric acid were weighed by weight, and steps S1 and S2 in Example 1 were carried out. The obtained molten liquid was poured onto the surface of a horizontally placed stainless steel plate while hot, and allowed to cool naturally in the air.
[0086] The difference between Comparative Example 5 and Example 3 is that the ratios of the raw materials used to prepare the slurry are different.
[0087] Comparative Example 6
[0088] 20 parts of gallium oxide, 26 parts of niobium oxide, 16 parts of cerium oxide and 30 parts of boric acid were weighed by weight, and steps S1 and S2 in Example 1 were carried out. The obtained molten liquid was poured onto the surface of a horizontally placed stainless steel plate while hot, and allowed to cool naturally in the air to obtain a solid.
[0089] The difference between Comparative Example 6 and Example 3 is that the raw material tungsten oxide is replaced by gallium oxide.
[0090] Comparative Example 7
[0091] Weigh 20 parts of tungsten oxide, 26 parts of niobium oxide, 16 parts of cerium oxide, and 30 parts of boric acid, and carry out step S1 in Example 1. Put the obtained precursor powder into a corundum crucible, raise the temperature from 50°C to 1500°C over 4 hours, and then keep it at 1500°C for 4 hours to obtain a molten liquid. Pour the molten liquid on the surface of a horizontally placed stainless steel plate while it is hot, and let it cool naturally in the air.
[0092] The difference between Comparative Example 7 and Example 3 is that the sintering procedure is different.
[0093] The morphologies of the samples obtained in Example 3 and Comparative Examples 4-6 were observed, and the refractive indices of the samples were tested using an ellipsometer. The results are shown in Table 2.
[0094] Table 2
[0095] Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 form Uniform and transparent Opaque, internal crystallization Opaque, internal crystallization Opaque, internal crystallization Opaque, internal crystallization Refractive Index 2.5 1.8 1.6 2.0 2.2
[0096] According to Table 2, whether a uniform and stable glass structure can be sintered is related to the raw materials, proportions and heating program of the slurry.
[0097] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a slurry for rare earth-based high band gap fillers for radiant cooling coatings, It is characterized in that The following steps are involved: S1. In parts by weight, 20-35 parts of tungsten oxide, 25-36 parts of niobium oxide, 13-20 parts of rare earth oxides and 16-35 parts of boron oxide are fully mixed and then ball milled and powdered to obtain a precursor powder; S2. The precursor powder is smelted and sintered to obtain a molten liquid; S3. The molten liquid was poured into cold water and quenched, and after filtering and drying, a powder A was obtained; S4. A liquid reagent was added to the powder A to prepare a mixed solution, and a dispersant was added to the mixed solution and then sand-milled to obtain slurries A1, A2, and A3 with different median particle sizes; S5. The slurry A1, A2 and A3 are mixed uniformly in proportion to obtain a product slurry; Wherein, the rare earth oxide comprises cerium oxide or lanthanum oxide; In step S2, the smelting and sintering process includes five stages, specifically: In the first stage, the temperature was raised evenly from 50°C to 400°C, and the heating time was 35 minutes; The second stage was kept at 400°C for 30 min; In the third stage, the temperature is evenly increased from 400°C to 900°C, and the heating time is 60 minutes; In the fourth stage, the temperature is evenly increased from 900°C to 1400°C, and the heating time is 120 min; The fifth stage is kept at 1400°C for 240 min; When the fifth step is performed, after keeping the temperature for 180 minutes, the material liquid is stirred at a speed of 60 r / min for 30 minutes, and then the temperature is kept until the sintering is completed; In step S4, the median particle size of the slurry A1 is 15-25 μm, the median particle size of the slurry A2 is 1-7 μm, and the median particle size of the slurry A3 is 0.3-0.7 μm; In step S5, the mass ratio of the slurries A1, A2 and A3 is 1:0.8-1.3:0.4-0.
6.
2. A method for preparing a slurry for rare earth-based high band gap fillers for radiant cooling coatings according to claim 1, It is characterized in that In step S1, the ball milling is performed using a planetary ball mill, the rotation speed of the ball mill is 400 r / min, the ratio of large, medium and small balls is 3:4:3, the volume ratio of air, liquid and balls in the ball milling chamber is 1:1:1, and the ball milling time is 12 h.
3. A method for preparing a slurry for rare earth-based high band gap fillers for radiant cooling coatings according to claim 1, It is characterized in that In step S4, the liquid reagent includes water or butyl acetate, and the content of the powder A in the mixed liquid is 40%.
4. The method for preparing a slurry for rare earth-based high band gap fillers for radiant cooling coatings according to claim 1, It is characterized in that In step S4, the dispersant includes BYK111 type dispersant, and the added amount of the dispersant is 12-15% of the mass of the mixed liquid.
5. A slurry for rare earth-based high band gap fillers for radiant cooling coatings obtained according to the preparation method according to any one of claims 1 to 4.
6. Use of the slurry according to claim 5 in preparing a radiation cooling coating.