Infrared stealth coating and preparation method thereof
Through the compounding and acid treatment technology of doped metal semiconductors and nanomaterials, the problem of the small absorption range of the infrared band of infrared stealth coatings is solved, and broad-spectrum absorption of the infrared band is achieved, as well as the long life and good mechanical properties of the coating film.
Patent Information
- Application Number
- CN202410220071.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-02-28
AI Technical Summary
Existing infrared stealth coatings have a small infrared band absorption range, resulting in poor infrared stealth performance.
Doped metal semiconductor materials and nanomaterials are used to form fillers. Through compounding and dispersing agents, thickeners, leveling agents, defoaming agents and film-forming additives, the dispersion and stability of the fillers are improved, and Nanomaterials are processed by acid etching to expand the layer spacing or tubular cavity and increase the loading efficiency of tin-doped indium oxide semiconductors.
It significantly improves the absorption capacity of the infrared band, extends the service life of the coating film, improves the mechanical properties and flame retardant properties of the coating film, and achieves the stealth effect of a wider infrared band.
Smart Images

Figure BDA0004717858530000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of infrared stealth coatings, and more specifically, to an infrared stealth coating and a preparation method thereof. Background Art
[0002] Stealth coating is a mysterious member of the coating family. It is not the "invisibility" in science fiction works, but a combination of skills and techniques in military terms to control the observability of the target or the characteristic signal of the target. At present, common stealth coatings include radar stealth coatings, infrared stealth coatings, laser stealth coatings, visible light stealth coatings, and new stealth coatings that have attracted more attention in recent years, such as multi-band absorbing materials, nano-layer materials, chiral absorbing materials, conductive polymer materials, plasma stealth materials, etc. Among them, the most commonly used stealth material is infrared stealth coating. Its main principle is to attenuate and absorb the infrared radiation energy of the target by improving the structural design and applying the infrared physics principle, which can make it difficult for infrared detection equipment to detect the target. Foreign infrared stealth technology has developed rapidly, and the infrared stealth coating products developed have been used in aviation equipment and ground weapons and equipment, and have achieved good results. Domestic research and development of infrared stealth coatings is also relatively rapid, and breakthroughs have been made in infrared stealth coatings. Infrared stealth coating is the most important type of thermal stealth material at present because of its simple process, convenient construction, durability and low cost. Most of the thermal stealth materials developed and applied so far belong to this category.
[0003] A Chinese patent with publication number CN109836997A mentions an infrared stealth coating and its preparation method. The application uses self-made composite glass ceramics as fillers, combined with polyurethane modified silicone resin and other materials, to effectively improve the structural strength, wear resistance and infrared stealth performance of the infrared stealth coating. However, the composite glass ceramic material silicon dioxide used as the main glass-forming oxide and also as a component of the infrared stealth coating can only absorb infrared light in some bands. In the field of infrared absorption spectrum, its absorption peak range is mainly concentrated in 1000-1200cm -1 , 800~900cm -1 , and 400~600cmcm -1 Region, relatively limited frequency band range.
[0004] In recent years, nanomaterials are materials with special structures and properties, which have been widely used in various fields. Among them, the stealth principle and application of nanomaterials is a topic that has attracted much attention. The stealth principle of nanomaterials is mainly based on the principles of optics, electromagnetics and acoustics, and achieves stealth effect by absorbing, scattering and reflecting incident light, electromagnetic waves or sound waves.
[0005] A Chinese patent with the authorization publication number "CN104260514B" discloses a method for preparing a highly conductive carbon nanotube paper composite material with infrared stealth and lightning protection performance and its application. The method involves purchasing multi-walled or single-walled nanotubes commonly found on the market, dispersing them through a series of dispersing methods, and then preparing nanopaper through reduced pressure suction filtration. The nanopaper is soaked in silver nitrate solutions of different concentrations, and the nanotubes have a large specific surface area to adsorb silver nitrate. The nanopaper is irradiated under a fluorescent lamp to decompose the adsorbed silver nitrate to produce silver particles, thereby improving the conductivity of the nanopaper. The high conductivity is conducive to absorbing light in the infrared band, and the high conductivity can be used as a conductor to increase the conduction rate of the instantaneous current. However, the carbon nanotubes in the application have not been treated, so the adsorption performance is low. Therefore, the silver nitrate loaded is less, the conductivity is relatively low, and the absorption of the infrared band is reduced.
[0006] In view of the above problems, it is necessary to provide an infrared stealth coating with wider infrared band absorption and better stealth performance. Summary of the invention
[0007] In order to improve the problem of small infrared band absorption range and poor infrared stealth performance of infrared stealth coatings in related technologies, the present application provides an infrared stealth coating and a preparation method thereof.
[0008] In a first aspect, the present application provides an infrared stealth coating, which adopts the following technical solution: an infrared stealth coating, comprising the following raw materials in percentage by weight:
[0009] 40-55wt% organic binder, 15-25wt% filler, 5-10wt% pigment, 0.2-3wt% dispersant, 0.2-3wt% thickener, 0.2-1.5wt% leveling agent, 0.2-0.8wt% defoamer, 0.2-0.8wt% film-forming aid, and the balance is water, wherein the filler is formed by doping metal semiconductor material and nanomaterial;
[0010] In a specific embodiment, the doped metal semiconductor material is a tin-doped indium oxide semiconductor filler;
[0011] In a specific embodiment, the nanomaterial is a tubular structure or a layered structure material, including one or more of carbon nanotubes, halloysite nanotubes and montmorillonite;
[0012] In a specific embodiment, the method for preparing the filler comprises the following steps:
[0013] a: The nanomaterial and nitric acid are mixed in a mass ratio of 1:(2-3), stirred for 2-3 hours, then vacuum filtered and washed, and the vacuum filtration and washing are repeated 2-4 times, and the obtained solid is dried for 4-5 hours to obtain sample a;
[0014] b: mixing sample a and a doped metal semiconductor material in a mass ratio of 1:(2-3) to obtain a mixture b, and then adding the mixture into water, wherein the mass ratio of water to the mixture b is controlled to be (4-5):1 to obtain a mixed solution c;
[0015] c: ultrasonically disperse the mixed solution c for 15 to 30 minutes, stir for 2 to 3 hours, then vacuum filter and wash, repeat the vacuum filtration and washing for 2 to 4 times, and dry the obtained solid for 4 to 5 hours to obtain the filler;
[0016] In a specific embodiment, the organic binder includes one or both of epoxy resin and polyurethane, and the pigment is a metal oxide;
[0017] In a specific embodiment, the dispersant includes one or more of polyoxyethylene stearyl alcohol ether, polysorbate, polyvinyl alcohol, and polycarboxylic acid;
[0018] In a specific embodiment, the dispersant includes polyoxyethylene stearyl alcohol ether;
[0019] In a specific embodiment, the thickener includes one or more of sodium fatty acid, potassium fatty acid, fatty acid ethanolamine, polyamide fatty acid sodium and polyamide fatty acid potassium;
[0020] In a specific embodiment, the thickener includes fatty acid ethanolamine;
[0021] In a specific embodiment, the leveling agent includes one or more of polydimethylsiloxane, polymethylphenylsiloxane, propylene glycol, glycerol and butylene glycol;
[0022] In a specific embodiment, the leveling agent includes polydimethylsiloxane;
[0023] In a specific embodiment, the film-forming aid includes one or more of N,N-dimethylacetamide, 6,6-dimethyl-3-azabicyclo[3.1.0]hexane, triethylene glycol monobutyl ether, and ethylene glycol monomethyl ether;
[0024] In a specific embodiment, the film-forming aid includes N,N-dimethylacetamide
[0025] In a specific embodiment, the defoamer includes one or more of an organosilicon defoamer, a polyether defoamer, a polyester defoamer, a polyurethane defoamer, and a polyvinyl alcohol defoamer;
[0026] In a specific embodiment, the defoaming agent includes a silicone defoaming agent.
[0027] In a second aspect, the present application provides a method for preparing an infrared stealth coating, which adopts the following technical solution:
[0028] A method for preparing an infrared stealth coating comprises the following steps:
[0029] S1. Weigh the pigment, dispersant, thickener, leveling agent, defoamer, film-forming agent and water by weight and mix them evenly to obtain liquid A;
[0030] S2. Weigh the organic binder by weight percentage and mix it evenly with liquid A to obtain liquid B;
[0031] S3. Weigh the filler according to the weight percentage and mix it evenly with liquid B to obtain the infrared stealth coating.
[0032] This application has the following beneficial effects:
[0033] (1) The present application compounds the doped metal semiconductor material and the nanomaterial by compounding the filler, and improves the dispersibility and stability of the filler in the organic binder by using a dispersant, a thickener, a leveling agent, a defoamer and a film-forming aid;
[0034] (2) The tin-doped indium oxide semiconductor in the filler of the present application has a relatively high infrared light absorption capacity in different bands due to its conductive and optical absorption properties, especially in the mid-infrared band. Since the resistivity of tin-doped indium oxide is relatively low, it can absorb more infrared light;
[0035] (3) The tubular or layered structure of the nanomaterial in the filler of the present application can load tin-doped indium oxide semiconductors, so that the material slowly releases tin-doped indium oxide during long-term use, thereby extending the service life of the stealth coating, which has high economic value and practical significance. The nano-tubular or layered material in the filler of the present application is further acid-etched. On the basis of the original, the loading efficiency of the tin-doped indium oxide semiconductor is further increased by expanding the interlayer spacing or the capacity of the tubular cavity, thereby extending the service life of the coating.
[0036] (4) The use of tin-doped indium oxide semiconductor and nanomaterial composite materials in the filler itself can also improve the mechanical properties and flame retardant properties of the coating. DETAILED DESCRIPTION
[0037] The present application is further described in detail below with reference to the embodiments.
[0038] Infrared stealth material is a special material that can effectively absorb, reflect or scatter infrared radiation wavelengths to achieve the purpose of stealth. Infrared stealth materials are widely used in military, aviation, aerospace, automobile and construction fields, and have important strategic significance and application value. Therefore, developing a coating with high stealth performance has high practical significance both in the military field and other fields. Through retrieval and repeated experiments, the applicant found that tin-doped indium oxide semiconductor can be used as an infrared absorption material with good performance of absorbing mid-infrared spectrum, and can absorb 1400nm~3000nm. At the same time, the applicant also found that some layered or tubular nanomaterials can adsorb some small molecules and slowly release the small molecules during use, in order to extend the performance of the coating. However, during the experiment, it was found that the adsorption effect of natural layered or tubular nanomaterials was not very ideal. This may be because the natural materials have not undergone any treatment, and other substances already exist in their layered or tubular structures, resulting in unsatisfactory adsorption effect when adsorbing the tin indium oxide semiconductor of this application. Therefore, the applicant further acid-treated the nanomaterials. The test results show that the adsorption effect is significantly increased. At the same time, it is also found that the mechanical properties and flame retardant properties of the coating are also improved.
[0039] The scheme of the present application is further explained below in conjunction with specific preparation examples.
[0040] Preparation Example
[0041] Preparation Example 1
[0042] This preparation example provides a method for preparing a tin-doped indium oxide semiconductor filler, which specifically includes the following steps:
[0043] Step 1: Weigh InCl3·5H2O and SnCl3·5H2O, and control the mass ratio of InCl3·5H2O to SnCl3·5H2O to be 20:1; add them into deionized water, wherein the mass ratio of the mixture of the two to water is 1:5, and stir them magnetically for 1 hour at room temperature at a speed of 400r / min until they are completely dissolved;
[0044] Step 2: Add polyethylene glycol to the solution prepared in the first step, wherein the mass ratio of polyethylene glycol to the solution prepared in the first step is 4:1; heat in a water bath, control the temperature to 55°C, and the speed to 400r / min. During this period, adjust the pH to 9 with ammonia water, stir for 3 hours, and completely precipitate;
[0045] Step 3: The precipitate from step 2 was vacuum filtered for 12 min, then washed with deionized water, and the filtration and washing were repeated 3 times. The obtained solid was dried in a drying oven at 110°C for 5 h.
[0046] Step 4: Transfer the dried solid obtained in step 3 to a muffle furnace and calcine at 750°C for 1.5 h, cool to room temperature, and take out the sample;
[0047] Step 5: Add the sample from step 4 into a ball mill and mill it to an average particle size of 40 μm as a spare sample.
[0048] The average molecular weight of the polyethylene glycol in this preparation example is 400, and the three substances InCl3·5H2O and SnCl3·5H2O are purchased through the Aladdin reagent platform.
[0049] Preparation Example 2
[0050] This preparation example provides a tin-doped indium oxide semiconductor prepared in the nanomaterial-loaded preparation example 1, and the specific steps are as follows:
[0051] Carbon nanotubes loaded with tin-doped indium oxide semiconductor:
[0052] Carbon nanotubes and tin-doped indium oxide semiconductors were added to deionized water at a mass ratio of 1:3, wherein the total mass ratio of deionized water to carbon nanotubes and tin-doped indium oxide semiconductors was controlled to be 5:1, and then ultrasonically dispersed at room temperature for 20 minutes, and then stirred at room temperature for 2.5 hours. The obtained sample was vacuum filtered for 15 minutes, and then washed with deionized water, and the vacuum filtration and washing were repeated 3 times. The obtained solid was dried in a drying oven at 110°C for 4.5 hours, and marked as sample 1;
[0053] Using the same method, halloysite nanotubes loaded with tin-doped indium oxide semiconductors were prepared, labeled as sample 2, and montmorillonite loaded with tin-doped indium oxide semiconductors were prepared, labeled as sample 3.
[0054] Preparation Example 3
[0055] This preparation example provides a method of treating carbon nanotubes, halloysite nanotubes and montmorillonite with nitric acid and then loading tin-doped indium oxide semiconductors. The specific steps are as follows:
[0056] The carbon nanotubes were treated with a 2 mol / L nitric acid solution, wherein the mass ratio of the nitric acid solution to the carbon nanotubes was controlled to be 2:1, and stirred at room temperature for 2.5 hours. The obtained sample was vacuum filtered for 15 minutes, and then washed with deionized water, and the vacuum filtration and washing were repeated 3 times. The obtained solid was dried in a drying oven at 110°C for 4.5 hours. Subsequently, the method of Preparation Example 2 was used to load the tin-doped indium oxide semiconductor, and the obtained sample was labeled as 11.
[0057] Using the same method, halloysite nanotubes loaded with tin-doped indium oxide semiconductors were prepared, labeled as sample 21, and montmorillonite loaded with tin-doped indium oxide semiconductors were prepared, labeled as sample 31.
[0058] Example
[0059] Example 1
[0060] S1. 7wt% pigment, 1.4wt% dispersant, 1.5wt% thickener, 0.9wt% leveling agent, 0.5wt% defoamer, 0.5wt% film-forming aid and 22.2wt% water were weighed and mixed, ultrasonically dispersed at room temperature for 30min, and then stirred at room temperature for 0.5h, with the speed controlled at 400r / min to obtain liquid A;
[0061] S2 weighed 46wt% organic binder by weight percentage, mixed with liquid A, stirred at room temperature for 0.5h, the speed was controlled at 300r / min, to obtain liquid B;
[0062] S3. Weigh 20 wt% of the filler according to weight percentage, mix it with liquid B, stir it at room temperature for 1 hour, and control the speed at 400 r / min to obtain the infrared stealth coating of the present application.
[0063] The organic adhesive selected in this embodiment is epoxy resin and polyurethane compounded in a mass ratio of 2:3; the filler selected is samples 11, 21 and 31 in Preparation Example 3 compounded in a mass ratio of 1:1:1; the pigment selected is zinc oxide; the dispersant selected is polyoxyethylene stearyl ether-10; the thickener selected is fatty acid diethanolamine; the leveling agent selected is polydimethylsiloxane; the film-forming aid selected is N,N-dimethylacetamide; the defoaming agent selected includes a silicone defoaming agent, and the above additives are all purchased.
[0064] Among them, polyoxyethylene stearyl ether-10, polydimethylsiloxane and silicone defoamer were all purchased from Aladdin reagent platform, polyurethane was non-ionic water-based polyurethane resin PU-8160A, purchased from Guangzhou Huitu New Materials Co., Ltd., and epoxy resin was epoxy resin E44, purchased from Changzhou Lebang Composite Materials Co., Ltd.
[0065] Example 2
[0066] S1. Weigh 5wt% pigment, 0.2wt% dispersant, 3wt% thickener, 0.2wt% leveling agent, 0.7wt% defoamer and 0.8wt% film-forming aid and 23.1wt% water by weight, mix, ultrasonically disperse at room temperature for 30min, then stir at room temperature for 0.5h, the speed is controlled at 400r / min, to obtain liquid A;
[0067] S2 weighed 42wt% organic binder by weight percentage, mixed with liquid A, stirred at room temperature for 0.5h, the speed was controlled at 400r / min, to obtain liquid B;
[0068] S3. Weigh 25 wt% of the filler according to weight percentage, mix it with liquid B, stir it at room temperature for 1 hour, and control the speed at 400 r / min to obtain the infrared stealth coating of the present application.
[0069] The components of this embodiment are the same as those of embodiment 1, and the main difference is that the dosage of each component is different.
[0070] Example 3
[0071] S1. Weigh 6wt% pigment, 1wt% dispersant, 2.6wt% thickener, 0.7wt% leveling agent, 0.2wt% defoamer and 0.3t% film-forming aid and 23.2wt% water by weight, mix, ultrasonically disperse at room temperature for 30min, then stir at room temperature for 0.5h, the speed is controlled at 400r / min, to obtain liquid A;
[0072] S2 weighed 44wt% organic binder by weight percentage, mixed with liquid A, stirred at room temperature for 0.5h, the speed was controlled at 300r / min, to obtain liquid B;
[0073] S3. Weigh 22 wt% of filler by weight, mix with liquid B, stir at room temperature for 1 h, and control the rotation speed at 400 r / min to obtain the infrared stealth coating of the present application.
[0074] The components of this embodiment are the same as those of embodiment 1, and the main difference is that the dosage of each component is different.
[0075] Example 4
[0076] S1. 8wt% pigment, 1.9wt% dispersant, 1.7wt% thickener, 1.2wt% leveling agent, 0.8wt% defoamer and 0.6wt% film-forming aid and 20.8wt% water were weighed and mixed, ultrasonically dispersed at room temperature for 30min, and then stirred at room temperature for 0.5h, with the speed controlled at 400r / min to obtain liquid A;
[0077] S2 weighed 46wt% organic binder by weight percentage, mixed with liquid A, stirred at room temperature for 0.5h, the speed was controlled at 500r / min, to obtain liquid B;
[0078] S3. Weigh 19 wt% of the filler according to weight percentage, mix it with liquid B, stir it at room temperature for 1 hour, and control the speed at 400 r / min to obtain the infrared stealth coating of the present application.
[0079] The components of this embodiment are the same as those of embodiment 1, and the main difference is that the dosage of each component is different.
[0080] Example 5
[0081] S1. Weigh 9wt% pigment, 2.5wt% dispersant, 0.8wt% thickener, 0.9wt% leveling agent, 0.6wt% defoamer and 0.2wt% film-forming aid and 19wt% water by weight, mix, ultrasonically disperse at room temperature for 30min, then stir at room temperature for 0.5h, control the speed at 400r / min, to obtain liquid A; S2. Weigh 50wt% organic binder by weight, mix with liquid A, stir at room temperature for 0.5h, control the speed at 400r / min, to obtain liquid B;
[0082] S3. Weigh 17 wt% of filler by weight, stir at room temperature for 1 hour, and control the rotation speed at 400 r / min to obtain the infrared stealth coating of the present application.
[0083] The components of this embodiment are the same as those of embodiment 1, and the main difference is that the dosage of each component is different.
[0084] Example 6
[0085] S1. 10wt% pigment, 3wt% dispersant, 0.2wt% thickener, 1.5wt% leveling agent, 0.4wt% defoamer and 0.7wt% film-forming aid and 14.2wt% water were weighed and mixed, ultrasonically dispersed at room temperature for 30min, and then stirred at room temperature for 0.5h, with the speed controlled at 400r / min to obtain liquid A;
[0086] S2 weighed 55wt% organic binder by weight percentage, mixed with liquid A, stirred at room temperature for 0.5h, the speed was controlled at 600r / min, to obtain liquid B;
[0087] S3. Weigh 15 wt% of the filler according to weight percentage, mix it with liquid B, stir it at room temperature for 1 hour, and control the speed at 400 r / min to obtain the infrared stealth coating of the present application.
[0088] The components of this embodiment are the same as those of embodiment 1, and the main difference is that the dosage of each component is different.
[0089] Example 7
[0090] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is sample 11 in preparation example 3.
[0091] Example 8
[0092] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is sample 21 in preparation example 3.
[0093] Example 9
[0094] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is sample 31 in preparation example 3.
[0095] Example 10
[0096] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is sample 1 in preparation example 2.
[0097] Embodiment 11
[0098] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is sample 2 in preparation example 2.
[0099] Example 12
[0100] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is sample 3 in preparation example 2.
[0101] Embodiment 13
[0102] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is samples 1, 2 and 3 in preparation example 2, compounded in a mass ratio of 1:1:1.
[0103] Embodiment 14
[0104] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is samples 21 and 31 in preparation example 3, compounded in a mass ratio of 1:1.
[0105] Embodiment 15
[0106] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is samples 11 and 31 in preparation example 3, compounded in a mass ratio of 1:1.
[0107] Example 16
[0108] The main difference between this embodiment and embodiment 1 is that the filler selected in this embodiment is the sample 11 and the sample 21 in the preparation example 3, which are compounded in a mass ratio of 1:1.
[0109] Comparative Example 1
[0110] The main difference between this comparative example and Example 1 is that the filler selected in this example is the tin-doped indium oxide semiconductor of Preparation Example 1.
[0111] Comparative Example 2
[0112] The main difference between this comparative example and Example 1 is that the filler selected in this example is carbon nanotube material.
[0113] Performance Testing
[0114] The performance of the products obtained in the above preparation examples and embodiments was tested
[0115] 1. Thermogravimetric analysis (TGA) was performed on Sample 1, Sample 2 and Sample 3 of Preparation Example 2 and Sample 11, Sample 21 and Sample 31 of Preparation Example 3 to calculate the loading amount of the tin-doped indium oxide semiconductor filler. The model of the instrument is MN33-TG 209F3. The results are shown in Table 1.
[0116] Table 1
[0117] sample Sample 1 Sample 2 Sample 3 Sample 11 Sample 21 Sample 31 Loading capacity (%) 25.6 29.1 27.5 32.8 35.4 33.7
[0118] 2. Infrared emissivity is one of the important indicators for evaluating the performance of stealth materials. By testing with an infrared radiation instrument, the infrared emissivity of the stealth material can be obtained and its performance can be evaluated. When conducting the test, attention should be paid to issues such as sample preparation, instrument calibration, and test environment to ensure the accuracy and reliability of the test results. By testing the infrared emissivity of stealth materials, important reference data can be provided for the research and development and application of stealth materials. Therefore, the samples prepared in Examples 1 to 16 and Comparative Examples 1-2 were respectively coated on 4cm*4cm aluminum alloy substrates by spraying, spraying 3 times, with an interval of 40min between each spray, and a spraying amount of 0.05L / m 2 , refer to HB20540-2018 to test the infrared emissivity, and test the infrared emissivity in the bands of 1000nm~1200nm and 1400nm~3000nm. The results are shown in Table 2.
[0119] Table 2
[0120]
[0121]
[0122] 3. The hardness of the paint films of Examples 1 to 16 and Comparative Examples 1 to 2 was tested by pencil hardness test, with reference to ASTM D3363-2005 "Standard test method for determination of coating hardness by pencil test method". The wear resistance of the coating films was tested with reference to GB / T 1768-2023 at 500 rd. The results are shown in Table 3.
[0123] Table 3
[0124] Example hardness Wear resistance Example 1 4H 600r Example 2 4H 570r Example 3 4H 590r Example 4 4H 580r Example 5 4H 580r Example 6 4H 590r Example 7 4H 560r Example 8 4H 570r Example 9 4H 560r Example 10 3H 550r Embodiment 11 3H 560r Example 12 3H 540r Embodiment 13 4H 560r Embodiment 14 4H 570r Embodiment 15 4H 550r Example 16 4H 560r Comparative Example 1 H 500r Comparative Example 2 3H 530r
[0125] Result analysis:
[0126] Combining Preparation Examples 1 to 3 and Table 1, it can be seen that nanomaterials with tubular structures or layered structures can load the tin-doped indium oxide semiconductor filler prepared in the present application. The amount of tin-doped indium oxide semiconductor filler loaded by the untreated material is slightly lower. This may be because these nanomaterials are all natural materials. Before being treated, there are some other small molecular fillers in their tubes or between layers, occupying a certain space, resulting in a way to load more fillers. After acid treatment, some small molecular substances may react with H+, thereby eluting from the layers or tubes, increasing the space and providing space for loading more fillers.
[0127] It can be seen from Examples 1 to 5 and Tables 2 and 3 that within the parameter range set in the present application, the prepared coating has a low infrared emissivity, and its infrared emissivity is between 0.01 and 0.03 in the infrared bands of 1000 nm to 1200 nm and 1400 nm to 3000 nm. This may be because the metal in the tin-doped indium oxide semiconductor has a good infrared absorption effect, and therefore has a low reflectivity. Among them, the result of Example 1 is the best, and it may be that under this ratio of addition, the components in the infrared stealth material cooperate with each other to achieve a good stealth effect.
[0128] Combining the results of Example 1, Example 7-16, Comparative Examples 1-2, Table 2 and Table 3, it can be seen that the present application can achieve a good stealth effect through compounding between tin-doped indium oxide semiconductor and nanofiller, and can also greatly improve the wear resistance and hardness of the coating. Among them, the infrared emissivity of Comparative Example 1 is low, but the hardness and wear resistance of the coating are low. It may be that the paint film of Comparative Example 1 only adds tin-doped indium oxide semiconductor, and is not compounded with nanomaterials. Therefore, the tin-doped indium oxide semiconductor can absorb infrared light well, and then the infrared emissivity is low, but without the compounding of nanomaterials, the hardness and wear resistance of the coating are significantly reduced, but for aviation materials, the hardness and wear resistance of the coating are a relatively important measurement parameter. Comparative Example 2 only uses carbon nanotube material as filler, and the infrared emission is high, which may be because the pure nanomaterial has a relatively poor absorption effect on the infrared spectrum. Comparing Example 1 with Examples 7-9 and Examples 14-16, it can be seen that the infrared emissivity of Examples 7-9 and Examples 14-16 is slightly improved. This may be because some groups carried by these nanomaterials themselves can absorb infrared, and each nanomaterial carries different groups, so it can absorb infrared light of different bands. However, if one or two of them are missing, its absorption of infrared will decrease. Examples 10-13, it can be seen that the infrared emissivity of Examples 10-13 is higher than that of Example 1, and also higher than that of Examples 7-9 and Examples 14-16. This may be because the nanomaterials that have not been treated with acid have less tin-doped indium oxide semiconductor fillers loaded, so the absorption performance of infrared is significantly reduced.
[0129] In summary, the filler obtained by compounding tin-doped indium oxide semiconductor and tubular or layered nanomaterials in the present application, in combination with other ingredients, can achieve a good infrared absorption effect and is an ideal infrared stealth material. At the same time, the addition of nanomaterials improves the mechanical properties of the coating.
[0130] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An infrared stealth coating, It is characterized in that The raw materials include the following weight percentages: 40~55wt% organic binder, 15~25wt% filler, 5~10wt% pigment, 0.2~3wt% dispersant, 0.2~3wt% thickener, 0.2~1.5wt% leveling agent, 0.2~0.8wt% defoamer, 0.2~0.8wt% film-forming aid, and the balance is water; The preparation method of the filler comprises the following specific steps: Treating carbon nanotubes with a 2 mol / L nitric acid solution, wherein the mass ratio of the nitric acid solution to the carbon nanotubes is controlled to be 2:1, stirring at room temperature for 2.5 hours, vacuum filtering the obtained sample for 15 minutes, then washing with deionized water, repeating the filtration and washing three times, and drying the obtained solid in a drying oven at 110° C. for 4.5 hours to obtain carbon nanotubes treated with nitric acid, adding the carbon nanotubes treated with nitric acid and tin-doped indium oxide semiconductors to deionized water at a mass ratio of 1:3, wherein the total mass ratio of deionized water to the carbon nanotubes and the tin-doped indium oxide semiconductors is controlled to be 5:1, and then ultrasonically dispersing at room temperature for 20 minutes, then stirring at room temperature for 2.5 hours, vacuum filtering the obtained sample for 15 minutes, then washing with deionized water, repeating the filtration and washing three times, and drying the obtained solid in a drying oven at 110° C. for 4.5 hours to obtain carbon nanotube-loaded tin-doped indium oxide semiconductors, and preparing halloysite nanotube-loaded tin-doped indium oxide semiconductors and montmorillonite-loaded tin-doped indium oxide semiconductors by the same method; The filler is a mixture of carbon nanotube-loaded tin-doped indium oxide semiconductor, halloysite nanotube-loaded tin-doped indium oxide semiconductor, and montmorillonite-loaded tin-doped indium oxide semiconductor in a mass ratio of 1:1:
1.
2. An infrared stealth coating according to claim 1, It is characterized in that The organic binder includes one or both of epoxy resin and polyurethane, and the pigment is metal oxide.
3. The infrared stealth coating according to claim 1, It is characterized in that The dispersant is a nonionic dispersant, including one or more of polyoxyethylene stearyl alcohol ether, polysorbate, polyvinyl alcohol, and polycarboxylic acid.
4. The infrared stealth coating according to claim 1, It is characterized in that The thickener includes one or more of sodium fatty acid, potassium fatty acid, fatty acid ethanolamine, polyamide fatty acid sodium and polyamide fatty acid potassium.
5. The infrared stealth coating according to claim 1, It is characterized in that The leveling agent includes one or more of polydimethylsiloxane, polymethylphenylsiloxane, propylene glycol, glycerol and butylene glycol.
6. The infrared stealth coating according to claim 1, It is characterized in that The film-forming aid includes one or more of N,N-dimethylacetamide, 6,6-dimethyl-3-azabicyclo[3.1.0]hexane, triethylene glycol monobutyl ether, and ethylene glycol monomethyl ether.
7. A method for preparing an infrared stealth coating according to any one of claims 1 to 6, It is characterized in that The steps include: S1. Weigh the pigment, dispersant, thickener, leveling agent, defoamer, film-forming agent and water by weight and mix them evenly to obtain liquid A; S2. Weigh the organic binder by weight percentage and mix it evenly with liquid A to obtain liquid B; S3. Weigh the filler according to the weight percentage and mix it evenly with liquid B to obtain the infrared stealth coating.
Citation Information
Patent Citations
Preparation method and application of a highly conductive carbon nanotube paper composite material with infrared stealth and lightning protection performance
CN104260514B
Infrared stealth coating material and preparation method thereof
CN109836997A
Waterborne heat-insulating slurry and preparation method thereof, as well as waterborne heat-insulating glass coating and preparation method thereof
CN106752237A