A sample preparation method for characterizing the microstructure of chip wire bonding micro solder joints
Through the cold inlay technology of epoxy resin and curing agent and the step-by-step sample grinding method of optical microscope, the problem of difficult to characterize the structure changes of the semiconductor chip microsolder joints is solved, and the rapid, economical and efficient sample preparation is achieved, and the lead bonds are improved Compatible with product reliability.
Patent Information
- Application Number
- CN202311821444.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-27
AI Technical Summary
The prior art is difficult to effectively characterize and improve the structural changes of the wire bonded microsolder joints of semiconductor chips, resulting in insufficient product reliability, and conventional sample preparation methods are time-consuming, costly and complex in operation.
The mixture of epoxy resin and curing agent is used to perform cold insertion, and the samples are ground step by step under an optical microscope, and the samples are quickly and accurately ground to the cross-section of the micro-weld joints, simplifying operation and reducing equipment requirements.
It greatly shortens sample preparation time, improves success rate, reduces costs, meets the needs of micro-weld joint tissue structure observation and EBSD characterization, and improves the reliability of wire bonding products.
Smart Images

Figure HDA0004634084810000011 
Figure HDA0004634084810000012 
Figure HDA0004634084810000021
Abstract
Description
Technical Field
[0001] The invention relates to a sample preparation method for characterizing the micro solder joint structure of a chip lead bonding, and belongs to the technical field of material analysis characterization sample preparation. Background Art
[0002] Semiconductors are currently in the post-Moore era, and packaging technology has become a major aspect of electronic manufacturing. Advanced 5G communication technology and three-dimensional integrated circuits (3D-IC) in the era of big data have made microelectronic interconnection technology face a crucial challenge, that is, to develop finer pitch wire bonding interconnection technology for increasingly dense I / O. Wire bonding plays a key role in achieving electrical connection between semiconductor chips and pins / pads. At present, the biggest gap between domestic wire bonding products and foreign products is concentrated on the service reliability after bonding. The determining factor of reliability is the property change process of the bonded micro solder joint interface during service. Due to the special geometric structure of micro solder joints and the complexity of application scenarios, there are changes in current density, temperature, stress, and chemical concentration inside the solder joint during service. Bonded micro solder joints are subjected to electrical, thermal, and mechanical stress field coupling during service, so there are many failure forms of micro solder joints, such as: thickening of the interface intermetallic compound (IMC) layer, depletion of the chip under bump metal layer (UBM), Koch voids, electromigration, etc. Based on this, how to clearly explain and characterize the structural evolution between micro solder joints and chip interconnection layers is crucial to improving the reliability of wire bonding products in my country. However, since the solder joints of wire bonding are all micron-scale structures, it is difficult to obtain observation cross-sections using conventional sample preparation methods. Therefore, it is urgent to develop a micro solder joint sample preparation method suitable for characterizing the structural change process of chip wire bonding micro solder joints.
[0003] At present, the semiconductor industry usually adopts the method of combining grinding and polishing with X-ray three-dimensional microscope (X-ray) to observe the position of micro solder joints to prepare samples for the characterization of bonded micro solder joints. However, this equipment is expensive and complicated to operate, and conventional laboratories generally do not have this equipment. The disadvantage of using this equipment for observation is that the sample under the X-ray three-dimensional microscope has only a simple shape and no clear structural features, which is not conducive to observation and positioning during grinding and polishing. This method usually takes 1-2 weeks to complete the preparation of a single sample, and the success rate is low. In addition, in recent years, advanced electron microscopy technology has also been gradually applied to the characterization of micro solder joints, and focused ion beam cutting (FIB) can be used to prepare cross-sections of wire-bonded micro solder joints. However, in addition to the extremely high equipment cost, FIB technology also has high requirements for the operating ability of technicians (operators must be proficient in using electron microscopes for at least five years). After FIB cutting for cross-section sample preparation, the sample and the sample stage are at an angle of 54°. When the micro-solder joints need to be analyzed for grain orientation and stress, the spatial state of the sample does not meet the EBSD test conditions, and the EBSD probe and the sample cross-section observation position cannot correspond, so the corresponding electron backscatter diffraction (EBSD) characterization cannot be completed. Due to this technical difficulty, the current FIB technology can only be used to prepare ordinary morphological observation cross-sections of micro-solder joints, and it is impossible to further explore and characterize the structural evolution of micro-solder joints. In addition, FIB technology has high requirements for chip height and packaging. When the chip is packaged, the polymer plastic encapsulation material wrapped on the chip will volatilize in large quantities during FIB processing, affecting the electron microscope photography effect. Summary of the invention
[0004] In view of the problems of long time consumption, high cost and complex technical requirements, the present invention proposes a sample preparation method for characterizing the micro solder joint structure of chip lead bonding, that is, using a mixture of epoxy resin (such as bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin or glycidyl amine epoxy resin) and a curing agent (such as amine curing agent, acid anhydride curing agent or latent curing agent) to cold mount the chip sample, and maintaining the chip sample in a horizontal position during the cold mounting process, so that the general position of the micro solder joint in the cold mounted sample can be observed with the naked eye, and the position of the micro solder joint can be clearly observed using an optical microscope; during the grinding process, the sample can be quickly ground to a position close to the micro solder joint, and then through optical microscope observation, the time required for grinding to the micro solder joint position can be more accurately estimated, and the micro solder joint cross-sectional position can be accurately ground, thereby greatly shortening the sample preparation time and improving the sample preparation success rate. The method of the present invention takes a short time, has simple equipment and materials, is easy to operate, can promptly judge the position of the solder joint during grinding and polishing by naked eyes, and has a high success rate of sample preparation; the cross section obtained after sample preparation can simultaneously meet the requirements of the organizational cross section observation of conventional micro solder joints and the fine structure characterization of EBSD.
[0005] A sample preparation method for characterizing the microstructure of chip wire bonding micro solder joints, the specific steps are as follows:
[0006] (1) clamping and fixing the chip sample horizontally in the mold, wherein the chip sample is a debonded chip sample, and the exposed surface of the micro solder joint of the chip sample is clamped downward; the chip sample is an undebonded chip sample, and the marked surface of the chip sample is clamped downward, and the marked surface is the back of the exposed surface of the micro solder joint; adding an epoxy resin-curing agent mixture into the mold to submerge the chip sample and the clamp, and letting it stand to solidify to obtain a cold mounted sample;
[0007] (2) Grinding the cold mounted sample step by step using sandpaper of different mesh sizes: Under optical microscope observation, the cold mounted sample is initially ground to a distance of 0.8 to 1.2 mm from the negative end surface of the chip sample, and the negative end of the chip of the cold mounted sample is coarsely ground, finely ground, and polished to the cross-sectional position of the target micro-solder point, and the negative end of the chip of the cold mounted sample is covered with a traceless tape;
[0008] (3) The positive end of the cold mounted chip is coarsely ground until the metal end is exposed to obtain a chip bonding micro solder joint tissue sample; the coarse grinding can be performed using 240-mesh sandpaper;
[0009] (4) Use electron microscopy to observe and characterize the chip bonding micro solder joint tissue samples.
[0010] The epoxy resin in step (1) is bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin or glycidyl amine epoxy resin, and has a viscosity of 10 to 10000 mPa·s; the curing agent is an amine curing agent, an acid anhydride curing agent or a latent curing agent; in the epoxy resin-curing agent mixture, the epoxy resin accounts for 65% to 98.5% and the curing agent accounts for 1.5% to 35% in terms of mass percentage.
[0011] When the chip sample in step (1) is an un-debonded chip sample, the estimated micro solder joint position of the chip sample is marked at a distance of 1.9 to 2.1 mm from the positive terminal of the chip sample.
[0012] The chip sample is a debonded chip sample, and the specific method of step (2) of grinding the sample step by step is:
[0013] 1) Use 240-grit sandpaper to grind the sample to a distance of 0.8 to 1.2 mm from the negative end of the chip sample;
[0014] 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0015] 3) Use 1200-grit sandpaper to grind the sample until the negative end of the chip sample is observed to see the lead position;
[0016] 4) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the lead and pad positions;
[0017] 5) Use 4000-grit sandpaper to grind until a complete target micro-solder joint cross section appears on the negative end surface of the chip sample;
[0018] 6) Polish the target micro solder joint cross-section position on the negative end surface of the chip sample.
[0019] The chip sample is a non-debonded chip sample, and the specific method of step (2) of grinding the sample step by step is:
[0020] 1) Use 240-grit sandpaper to grind the sample to a distance of 0.8 to 1.2 mm from the negative end of the chip sample;
[0021] 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0022] 3) Use 1200-grit sandpaper to grind the sample until the negative end is 0.8 to 1.2 mm away from the chip sample mark position;
[0023] 4) Use 2000-grit sandpaper to grind the sample to the marked position on the negative end of the chip sample;
[0024] 5) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the lead and pad positions;
[0025] 6) Use 4000-grit sandpaper to grind until a complete target micro-solder joint cross section appears on the negative end of the chip sample;
[0026] 7) Polish the target micro solder joint cross-section position on the negative end surface of the chip sample.
[0027] The specific method of polishing in step (2) is:
[0028] 1) Use 2.5μm polishing paste for initial polishing until the number of scratches is no more than 30, the scratch depth is no more than 5μm, and the length is no more than 200μm;
[0029] 2) Use 1.5μm polishing paste to polish the sample micro solder joint several times until there are no scratches or the number of scratches is no more than 5, and the scratch depth is no more than 2μm and the length is no more than 50μm;
[0030] 3) Use clean water to micro-polish to remove the polishing paste on the surface of the micro-solder points.
[0031] The beneficial effects of the present invention are:
[0032] (1) The present invention uses a mixture of epoxy resin (such as bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin or glycidyl amine epoxy resin) and a curing agent (such as amine curing agent, acid anhydride curing agent or latent curing agent) to cold mount the chip sample, and maintains the chip sample in a horizontal position during the cold mounting process, so that the general position of the micro solder joints in the cold mounted sample can be observed with the naked eye, and the position of the micro solder joints can be clearly observed using an optical microscope; during the grinding process, the sample can be quickly ground to a position close to the micro solder joint, and then observed under an optical microscope, so that the time required for grinding to the micro solder joint position can be more accurately estimated, and the micro solder joint cross-sectional position can be accurately ground to improve the success rate of sample preparation;
[0033] (2) Unlike the traditional technology that requires repeated grinding and observation and replacement of finer sandpaper, the present invention only requires grinding to the vicinity of the micro-weld point once, and then slowly grinding to the cross-section of the micro-weld point. The number of grinding steps is greatly reduced, which can greatly shorten the sample preparation time;
[0034] (3) The method of the present invention only requires the use of an ordinary optical microscope and a grinder and polisher. It is easy to operate and does not require the use of high-end microscopic instruments (such as X-ray three-dimensional microscope (X-ray), ultrasonic scanning microscope). It has fewer requirements for instruments and reduces the cost of sample preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a sample diagram of the preparation process;
[0036] Figure 2 The sample pictures of the cold mounted samples after initial grinding in Examples 1 to 3;
[0037] Figure 3 The figure is a diagram of the grinding and polishing process of the chip bonding micro solder joints in Examples 1 to 3 under an optical microscope;
[0038] Figure 4 is a map of the marking positions on the chip sample in Example 3;
[0039] Figure 5 This is the sample picture after the cold mounted sample is completely ground and polished;
[0040] Figure 6 This is the morphology image of the cold-mounted sample of the bonding wire micro-solder joint in the implementation case after grinding and polishing under the electron microscope;
[0041] Figure 7 This is the EBSD image of the cold-mounted sample of the bonding wire micro-solder joint after grinding and polishing in the implementation case. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0043] Summary of the Invention
[0044] A sample preparation method for characterizing the microstructure of chip wire bonding micro solder joints, the specific steps are as follows:
[0045] (1) The chip sample is clamped and fixed horizontally in a mold, wherein the epoxy resin is bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin or glycidyl amine epoxy resin, and has a viscosity of 10 to 10000 mPa·s; the curing agent is an amine curing agent, an acid anhydride curing agent or a latent curing agent; in terms of mass percentage, the epoxy resin accounts for 65% to 98.5% of the epoxy resin-curing agent mixture, and the curing agent accounts for 1. 5% to 35%; if the chip sample is a debonded chip sample, the exposed surface of the micro solder joint of the chip sample is clamped downward; if the chip sample is an undebonded chip sample, the estimated micro solder joint position of the chip sample is marked at 1.9 to 2.1 mm away from the positive end of the chip sample, and the marked surface of the chip sample is clamped downward, and the marked surface is the back of the exposed surface of the micro solder joint; add the epoxy resin-curing agent mixture into the mold to submerge the chip sample and the fixture, and let it stand to solidify to obtain a cold mounted sample;
[0046] (2) Grinding the cold mounted sample step by step using sandpaper of different mesh sizes: Under optical microscope observation, the cold mounted sample is initially ground to a distance of 0.8 to 1.2 mm from the negative end surface of the chip sample, and the negative end of the chip of the cold mounted sample is coarsely ground, finely ground, and polished to the cross-sectional position of the target micro-solder point, and the negative end of the chip of the cold mounted sample is covered with a traceless tape;
[0047] If the chip sample is a debonded chip sample, cold mount the sample (see Figure 1 (a)) The specific method of grinding samples step by step is:
[0048] 1) Use 240-grit sandpaper to grind the sample to a distance of 0.8 to 1.2 mm from the negative end of the chip sample (see Figure 1 (b));
[0049] 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0050] 3) Use 1200-grit sandpaper to grind the sample until the negative end of the chip sample is observed to see the lead position;
[0051] 4) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the lead and pad positions;
[0052] 5) Use 4000-grit sandpaper to grind until the negative end of the chip sample has a complete target micro-solder point cross section (see Figure 1 (c));
[0053] 6) Polish the target micro solder joint cross-section position on the negative end surface of the chip sample.
[0054] If the chip sample is a non-debonded chip sample, the specific method of grinding the sample step by step is as follows:
[0055] 1) Use 240-grit sandpaper to grind the sample to a distance of 0.8 to 1.2 mm from the negative end of the chip sample;
[0056] 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0057] 3) Use 1200-grit sandpaper to grind the sample until the negative end is 0.8 to 1.2 mm away from the chip sample mark position;
[0058] 4) Use 2000-grit sandpaper to grind the sample to the marked position on the negative end of the chip sample;
[0059] 5) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the lead and pad positions;
[0060] 6) Use 4000-grit sandpaper to grind until a complete target micro-solder joint cross section appears on the negative end of the chip sample;
[0061] 7) Polish the target micro solder joint cross-section position on the negative end surface of the chip sample.
[0062] The specific method of the polishing is:
[0063] 1) Use 2.5μm polishing paste for initial polishing until the number of scratches is no more than 30, the scratch depth is no more than 5μm, and the length is no more than 200μm;
[0064] 2) Use 1.5μm polishing paste to polish the sample micro solder joint several times until there are no scratches or the number of scratches is no more than 5, and the scratch depth is no more than 2μm and the length is no more than 50μm;
[0065] 3) Use clean water micro-polishing to remove the polishing paste on the surface of the micro-solder points;
[0066] (3) The positive end of the cold mounted chip is roughly ground until the metal end is exposed to obtain the chip bonding micro solder joint tissue sample (see Figure 1 (d)); the rough grinding can be performed using 240 mesh sandpaper;
[0067] (4) Use electron microscopy to observe and characterize the chip bonding micro solder joint tissue samples.
[0068] Example 1: The chip sample in this example is a chip sample with debonding, and the direct observation method is adopted;
[0069] A sample preparation method for characterizing the microstructure of chip wire bonding micro solder joints, the specific steps are as follows:
[0070] (1) clamping and fixing a chip sample horizontally in a mold, wherein the chip sample is a debonded chip sample, and the exposed surface of the micro solder joint of the chip sample (the front of the chip sample) is clamped downward; the epoxy resin is a commercially available low-viscosity epoxy resin and polybutadiene peroxide, and the viscosity is 10 to 100 mPa·s, and the curing agent is triethylenetetramine; in terms of mass percentage, the low-viscosity resin accounts for 76.92% and the curing agent accounts for 23.08%; adding the epoxy resin-curing agent mixture into the mold to submerge the chip sample and the fixture, and letting it stand and solidify to obtain a cold mounted sample;
[0071] (2) Use sandpaper of different meshes to cold mount the specimens (see Figure 2 (a) Perform step-by-step sample grinding: Under optical microscope observation, the exposed surface of the micro solder joint and the negative terminal of the cold mounted chip sample are initially ground to a shape that is 1 mm away from the end face of the chip sample and is easy to observe; using water as a coolant, sandpaper of different meshes is used to coarsely grind, finely grind and polish the negative terminal of the cold mounted chip to the target micro solder joint cross-section position, and the negative terminal of the cold mounted chip is covered with a traceless tape;
[0072] The chip sample is a debonded chip sample, and the specific method of grinding the cold mounted sample step by step is as follows:
[0073] 1) Use water as the coolant and use 240-grit sandpaper to grind the sample to 1 mm from the negative end of the chip sample;
[0074] 2) Use water as the coolant and use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0075] 3) Use water as the coolant and use 1200-grit sandpaper to grind the sample until the negative end of the chip sample is observed. Figure 3 As shown in (a), the exposed surface of the micro solder joint (the front side of the chip sample) is Figure 3 (d)
[0076] 4) Use water as the coolant and use 2000-grit sandpaper to grind the sample until the negative end of the chip sample is observed. During the grinding process, observe the front side of the sample (the exposed surface of the micro solder joint) and the negative end of the sample through an optical microscope to determine the distance from the micro solder joint. Grind the sample to a position near the target micro solder joint. That is, the pad can be observed when observing the negative electrode of the sample under an optical microscope, and there is a little lead above the pad. Figure 3 (b)
[0077] 5) Use water as the coolant and 4000-grit sandpaper to grind the negative end of the chip sample until a complete target micro-solder point cross section appears. During the grinding process, an optical microscope can be used to observe that another point appears above the negative electrode pad of the sample, and the area of the two points becomes larger and larger until they are completely connected. Figure 3 As shown in (c), the front side of the sample (exposed side of the micro solder joint) is Figure 3As shown in (e), the complete negative end grinding process is completed;
[0078] The sample grinding process has a rotation speed of 200 r / min. During the sample grinding process, the sample needs to be observed and ground through an optical microscope. The main observation surfaces are the front side of the cold mounted sample (the exposed surface of the micro-weld point) and the negative end.
[0079] 6) Polishing the target micro solder joint cross-sectional position on the negative end surface of the chip sample; the specific method of polishing is:
[0080] 1) Use 2.5μm polishing paste for initial polishing until the number of scratches is no more than 30, and the scratch depth is no more than 5μm and the length is no more than 200μm to reduce scratches on the chip and micro solder joints;
[0081] 2) In the same direction, use 1.5μm polishing paste to polish the sample micro solder joint several times until there is no scratch on the cross section or the number of scratches is no more than 5, and the scratch depth is no more than 2μm and the length is no more than 50μm;
[0082] 3) Use clean water micro-polishing to remove the polishing paste on the surface of the micro-solder points;
[0083] The polishing process speed is 200r / min and the single polishing time does not exceed 3min;
[0084] (3) Use 240-grit sandpaper to coarsely grind the positive end of the cold-mounted chip until the metal end is exposed (the positive end of the sample shows metallic luster), and obtain the chip bonding micro-solder joint structure sample (see Figure 5 );
[0085] (4) Using electron microscopy to observe and characterize the microstructure samples of chip bonding micro solder joints;
[0086] The micro solder joint structure samples of the chip bonding in this embodiment were characterized by electron microscope observation, and clear micro solder joint cross-sectional morphological features were obtained. Figure 6 (a) shows; then the micro solder joint cross section is locally scanned by EBSD, the result is as follows Figure 7 (a) is shown; the figure can be used to analyze interface defects, grain orientation, grain boundary conditions and grain changes, etc., which can ultimately be used to determine the interface reaction mechanism of the bonding wire and analyze the interface conditions, providing a clear and complete micro-solder point cold-mounted sample and a reliable sample preparation method for the failure study of the bonding wire.
[0087] Example 2: The chip sample in this example is a chip sample with debonding, and the direct observation method is adopted;
[0088] A sample preparation method for characterizing the microstructure of chip wire bonding micro solder joints, the specific steps are as follows:
[0089] (1) clamping and fixing a chip sample horizontally in a mold, wherein the chip sample is a chip sample with glue removed, and the exposed surface of the micro solder joint of the chip sample (the front of the chip sample) is clamped and fixed downward, and the epoxy resin is a bisphenol A epoxy resin with a viscosity of 1000 to 10000 mPa·s, and the curing agent is polyethylene polyamine; in terms of mass percentage, the low-viscosity resin accounts for 94.74% and the curing agent accounts for 5.26%; adding the epoxy resin-curing agent mixture into the mold to submerge the chip sample and the clamp, and letting it stand and solidify to obtain a cold mounted sample;
[0090] (2) Use sandpaper of different meshes to cold mount the specimens (see Figure 2 (b) Perform step-by-step sample grinding: Under optical microscope observation, the exposed surface of the micro solder joint and the negative terminal of the cold mounted chip sample are initially ground to a shape that is 1 mm away from the end face of the chip sample and is easy to observe; using water as a coolant, sandpaper of different meshes is used to coarsely grind, finely grind and polish the negative terminal of the cold mounted chip to the target micro solder joint cross-section position, and the negative terminal of the cold mounted chip is covered with a traceless tape;
[0091] The chip sample is a debonded chip sample, and the specific method of grinding the cold mounted sample step by step is as follows:
[0092] 1) Use water as the coolant and use 240-grit sandpaper to grind the sample to 1 mm from the negative end of the chip sample;
[0093] 2) Use water as the coolant and use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0094] 3) Use water as the coolant and use 1200-grit sandpaper to grind the sample until the negative end of the chip sample is observed. Figure 3 As shown in (a), the exposed surface of the micro solder joint (the front side of the chip sample) is Figure 3 (d)
[0095] 4) Use water as the coolant and use 2000-grit sandpaper to grind the sample until the negative end of the chip sample is observed. During the grinding process, observe the front side of the sample (the exposed surface of the micro solder joint) and the negative end of the sample through an optical microscope to determine the distance from the micro solder joint. Grind the sample to a position near the target micro solder joint. That is, the pad can be observed when observing the negative electrode of the sample under an optical microscope, and there is a little lead above the pad. Figure 3 (b)
[0096] 5) Use water as the coolant and 4000-grit sandpaper to grind the negative end of the chip sample until a complete target micro-solder point cross section appears. During the grinding process, an optical microscope can be used to observe that another point appears above the negative electrode pad of the sample, and the area of the two points becomes larger and larger until they are completely connected. Figure 3 As shown in (c), the front side of the sample (exposed side of the micro solder joint) is Figure 3As shown in (e), the complete negative end grinding process is completed;
[0097] The sample grinding process has a rotation speed of 200 r / min. During the sample grinding process, the sample needs to be observed and ground through an optical microscope. The main observation surfaces are the front side of the cold mounted sample (the exposed surface of the micro-weld point) and the negative end.
[0098] 6) Polishing the target micro solder joint cross-sectional position on the negative end surface of the chip sample; the specific method of polishing is:
[0099] 1) Use 2.5μm polishing paste for initial polishing until the number of scratches is no more than 30, and the scratch depth is no more than 5μm and the length is no more than 200μm to reduce scratches on the chip and micro solder joints;
[0100] 2) In the same direction, use 1.5μm polishing paste to polish the sample micro solder joint several times until there is no scratch on the cross section or the number of scratches is no more than 5, and the scratch depth is no more than 2μm and the length is no more than 50μm;
[0101] 3) Use clean water micro-polishing to remove the polishing paste on the surface of the micro-solder points;
[0102] The polishing process speed is 200r / min and the single polishing time does not exceed 3min;
[0103] (3) Use 240-grit sandpaper to coarsely grind the positive end of the cold-mounted chip until the metal end is exposed (the positive end of the sample reveals metallic luster) to obtain a chip bonding micro-solder joint tissue sample;
[0104] (4) Using electron microscopy to observe and characterize the microstructure samples of chip bonding micro solder joints;
[0105] The micro solder joint structure samples of the chip bonding in this embodiment were characterized by electron microscope observation, and clear micro solder joint cross-sectional morphological features were obtained. Figure 6 (b) shows. Then perform a local EBSD scan on the micro solder joint cross section, and the results are shown in Figure 7 (b) As shown; the figure can be used to analyze interface defects, grain orientation, grain boundary conditions and grain changes, etc., which can ultimately be used to determine the interface reaction mechanism of the bonding wire and analyze the interface conditions, providing a clear and complete micro-solder point cold-mounted sample and a reliable sample preparation method for the failure study of the bonding wire.
[0106] Example 3: The chip sample in this example is a non-stripped chip sample, and the scale estimation method is used;
[0107] A sample preparation method for characterizing the microstructure of chip wire bonding micro solder joints, the specific steps are as follows:
[0108] (1) The chip sample is clamped and fixed horizontally in the mold. The chip sample is a chip sample without debonding. The micro solder joint position of the chip sample is estimated and marked using the scale method (the mark is located at a position 2 mm away from the positive electrode frame of the chip sample, see Figure 4 ), the marked surface of the chip sample is clamped downward, the marked surface is the back of the exposed surface of the micro solder joint, at this time, the front side of the chip sample (micro solder joint surface, but the micro solder joint is covered by colloid and cannot be observed) is upward, the epoxy resin is low-viscosity epoxy resin and peroxide polybutadiene, the viscosity is 10-100mPa·s, and the curing agent is triethylenetetramine; in terms of mass percentage, the low-viscosity resin accounts for 76.92%, and the curing agent accounts for 23.08%; the epoxy resin-curing agent mixture is added into the mold to submerge the chip sample and the fixture, and is allowed to stand and solidify to obtain a cold mounted sample;
[0109] (2) Use sandpaper of different meshes to cold mount the specimens (see Figure 2 (c) Grinding the sample step by step: Under optical microscope observation, the marked surface and the negative end of the cold mounted chip sample are initially ground to a distance of 1 mm from the end face of the chip sample to obtain a shape that is easy to observe; using water as a coolant, sandpaper of different meshes is used to coarsely grind, finely grind and polish the negative end of the cold mounted chip sample to the cross-sectional position of the target micro-solder point, and the negative end of the cold mounted chip sample is covered with a traceless tape;
[0110] The chip sample is a non-debonded chip sample, and the specific method of grinding the sample step by step is as follows:
[0111] 1) Use 240-grit sandpaper to grind the sample to 1 mm from the negative end of the chip sample;
[0112] 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample;
[0113] 3) Use 1200-grit sandpaper to grind the sample until the negative end is 1 mm away from the chip sample mark position;
[0114] 4) Use 2000-grit sandpaper to grind the sample to the marked position on the negative terminal of the chip sample. Observe the negative electrode of the sample under a light microscope to observe the lead. Figure 3 (a)
[0115] 5) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the position of the lead and pad; observe the negative electrode of the sample under a light microscope to observe the pad and a point above the pad as well as the unconnected lead. Figure 3 (b)
[0116] 6) Use 4000-grit sandpaper to grind until a complete target micro-solder point cross section appears on the negative end surface of the chip sample; during the grinding process, an optical microscope can be used to observe that another point appears above the negative electrode pad of the sample, and the area of the two points becomes larger and larger until they are completely connected. Figure 3(c) shows the complete negative end grinding process;
[0117] The sample grinding process has a rotation speed of 200 r / min. During the sample grinding process, the sample needs to be observed and ground through an optical microscope, and the main observation surface is the negative end of the cold mounted sample.
[0118] 7) Polishing the target micro solder joint cross-sectional position on the negative end surface of the chip sample; the specific method of polishing is:
[0119] 1) Use 2.5μm polishing paste for initial polishing until the number of scratches is no more than 30, and the scratch depth is no more than 5μm and the length is no more than 200μm to reduce scratches on the chip and micro solder joints;
[0120] 2) In the same direction, use 1.5μm polishing paste to polish the sample micro solder joint several times until there is no scratch on the cross section or the number of scratches is no more than 5, and the scratch depth is no more than 2μm and the length is no more than 50μm;
[0121] 3) Use clean water micro-polishing to remove the polishing paste on the surface of the micro-solder points;
[0122] The polishing process speed is 200r / min and the single polishing time does not exceed 3min;
[0123] (3) Use 240-grit sandpaper to coarsely grind the positive end of the cold-mounted chip until the metal end is exposed (the positive end of the sample shows metallic luster), and obtain the chip bonding micro-solder joint structure sample (see Figure 5 );
[0124] (4) Using electron microscopy to observe and characterize the microstructure samples of chip bonding micro solder joints;
[0125] The micro solder joint structure samples of the chip bonding in this embodiment were characterized by electron microscope observation, and clear micro solder joint cross-sectional morphological features were obtained. Figure 6 (c) shows; then the micro solder joint cross section is subjected to local EBSD scanning, and the results are shown in Figure 7 (c) As shown; the figure can be used to analyze interface defects, grain orientation, grain boundary conditions and grain changes, etc., which can ultimately be used to determine the interface reaction mechanism of the bonding wire and analyze the interface conditions, providing a clear and complete micro-solder point cold-mounted sample and a reliable sample preparation method for the failure study of the bonding wire.
[0126] The method of the present invention can complete the entire grinding and polishing process by using only an optical microscope during the sample grinding and polishing process, without using high-end microscope instruments in traditional grinding and polishing methods, which greatly reduces the sample preparation cost of the bonded micro-solder joint cross section. The sample preparation method of the present invention is simple to operate and takes a short time, which solves the problem of traditional technical methods requiring multiple instruments and long grinding and polishing time.
[0127] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing a sample to characterize the microstructure of a chip wire bonding micro solder joint, characterized in that: The specific steps are as follows: (1) Clamping and fixing the chip sample horizontally in the mold, wherein the chip sample is a debonded chip sample, and the exposed surface of the micro solder joint of the chip sample is clamped downward; clamping and fixing the chip sample horizontally in the mold, wherein the chip sample is an undebonded chip sample, marking the estimated micro solder joint position of the chip sample at a distance of 1.9 to 2.1 mm from the positive end of the chip sample, and clamping and fixing the chip sample with the marked surface downward, wherein the marked surface is the back of the exposed surface of the micro solder joint; adding the epoxy resin-curing agent mixture into the mold to submerge the chip sample and the fixture, and letting it stand to solidify to obtain a cold mounted sample; (2) Grind the cold mounted sample step by step using sandpaper of different mesh sizes: Under optical microscope observation, grind the cold mounted sample to a distance of 0.8-1.2 mm from the negative end surface of the chip sample, and perform coarse grinding, fine grinding and polishing on the negative end of the chip of the cold mounted sample to the cross-sectional position of the target micro-solder point. Cover the negative end of the chip of the cold mounted sample with a traceless tape; specifically, The chip sample is a chip sample with the glue removed, and the specific method of grinding the sample step by step is: 1) Use 240-grit sandpaper to grind the sample to 0.8-1.2 mm from the negative end of the chip sample; 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample; 3) Use 1200-grit sandpaper to grind the sample until the negative end of the chip sample is observed to see the lead position; 4) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the lead and pad positions; 5) Use 4000-grit sandpaper to grind until a complete target micro-solder joint cross section appears on the negative end of the chip sample; 6) The cross-sectional location of the target micro solder joint on the negative end of the polished chip sample; The chip sample is a non-debonded chip sample, and the specific method of grinding the sample step by step is as follows: 1) Use 240-grit sandpaper to grind the sample to 0.8-1.2 mm from the negative end of the chip sample; 2) Use 600-grit sandpaper to grind the sample to the negative end of the chip sample; 3) Use 1200-grit sandpaper to grind the sample until the negative end is 0.8-1.2 mm away from the chip sample mark position; 4) Use 2000-grit sandpaper to grind the sample to the marked position on the negative end of the chip sample; 5) Use 2000-grit sandpaper to grind the sample to the negative end of the chip sample to observe the lead and pad positions; 6) Use 4000-grit sandpaper to grind until a complete target micro-solder joint cross section appears on the negative end of the chip sample; 7) The cross-sectional location of the target micro solder joint on the negative end of the polished chip sample; The specific method of the polishing is: 1) Use 2.5μm polishing paste for initial polishing until the number of scratches is no more than 30, the scratch depth is no more than 5μm, and the length is no more than 200μm; 2) Use 1.5μm polishing paste to polish the sample micro solder joints several times until there are no scratches or the number of scratches is no more than 5, and the scratch depth is no more than 2μm and the length is no more than 50μm; 3) Use clean water micro-polishing to remove the polishing paste on the surface of the micro-solder points; (3) The positive end of the cold mounted chip is roughly ground until the metal end is exposed to obtain a chip bonding micro solder joint tissue sample; (4) Use electron microscopy to observe and characterize the microstructure samples of chip bonding micro solder joints.
2. The method for preparing a sample for characterizing the microstructure of a chip wire bonding micro solder joint according to claim 1, characterized in that: In step (1), the epoxy resin is a bisphenol A epoxy resin, a bisphenol F epoxy resin, an aliphatic glycidyl ether epoxy resin, a glycidyl ester epoxy resin or a glycidyl amine epoxy resin, and has a viscosity of 10 to 10000 mPa·s; the curing agent is an amine curing agent or an acid anhydride curing agent; in the epoxy resin-curing agent mixture, the epoxy resin accounts for 65% to 98.5% and the curing agent accounts for 1.5% to 35% by mass.
Citation Information
Patent Citations
Preparation method of electronic back scattering diffraction sample of tin-based solder interconnecting welding spot
CN108061737A
Evaluation method for bonding quality of bonding wire of semiconductor device
CN109632791A
Transmission electron microscope sample preparation method suitable for dissimilar material welding joint interface analysis
CN111624214A
Positioning method and positioning device for target position of semiconductor chip sample
CN111834273A
Manufacture technique of miniaturized shear-punchspecimen for solder joint
KR1020040075397A