Photosensitive dry film coating and preparation method thereof
By adjusting the ratio of alkali-soluble resin and photosensitive monomer, the problem of low resolution and insufficient adhesion of photosensitive dry film coating at high resolution is solved, achieving higher resolution and adhesion to meet the needs of high-precision manufacturing. .
Patent Information
- Application Number
- CN202410182686.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-02-19
AI Technical Summary
Existing photosensitive dry film coatings are prone to blurred lines, unclear edges, and insufficient adhesion under high resolution, making it difficult to meet the needs of high-precision manufacturing.
Alkali-soluble resin obtained by copolymerizing a variety of acrylic resin monomers is used, and by adjusting its ratio, combined with the compounding of multiple photosensitive monomers, propoxy groups and fluorine-containing segments are introduced to synergistically improve resolution and adhesion.
Significantly improves the resolution and adhesion of the photosensitive dry film, achieving clearer pattern formation and stronger substrate adhesion at high resolution.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a photosensitive dry film coating and a preparation method thereof. Background Art
[0002] Photosensitive dry film coating is one of the important functional materials in the electronics industry, and is widely used in the production of electronic circuit boards, printed circuit boards (PCBs), integrated circuit packaging, flat panel display production, etc. Photosensitive dry film coating has excellent photosensitivity and resolution, and can undergo chemical reactions under light conditions to form the desired pattern or circuit.
[0003] With the rapid development of the electronics industry, higher requirements are placed on photosensitive dry film coatings. Although the photosensitive dry film coatings currently on the market can meet basic production needs, there are still some technical problems that need to be solved. First of all, the resolution of photosensitive dry film coatings needs to be further improved. With the continuous miniaturization and integration of electronic products, the resolution requirements for photosensitive dry film coatings are getting higher and higher. However, existing photosensitive dry film coatings are prone to problems such as blurred lines and unclear edges at high resolutions, which makes it difficult to meet the needs of high-precision manufacturing. Secondly, the adhesion between the photosensitive dry film and the substrate also needs to be improved to prevent peeling between the photosensitive dry film and the substrate. In summary, as an important functional material in the electronics industry, photosensitive dry film coatings still face technical problems of low resolution and poor adhesion.
[0004] Therefore, in view of the above technical problems, developing a high-resolution and high-adhesion photosensitive dry film coating and a preparation method thereof has important practical significance and market value. The present invention aims to solve the above problems and provide a high-resolution and high-adhesion photosensitive dry film coating and a preparation method thereof. Summary of the invention
[0005] In view of the defects of the above-mentioned prior art, an object of the present invention is to provide a photosensitive dry film coating, aiming to solve the technical problems of insufficient resolution and poor adhesion of the existing photosensitive dry film coating.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A photosensitive dry film coating, comprising the following raw materials in parts by weight:
[0008] 40-70 parts of alkali soluble resin
[0009] Photosensitive monomer 20-50 parts
[0010] Photoinitiator 0.05-5 parts
[0011] 10-20 parts of solvent.
[0012] The alkali-soluble resin is an acrylic resin, specifically a copolymer obtained by polymerizing the following acrylic resin monomers: methyl methacrylate, styrene and hexafluorobutyl methacrylate.
[0013] The mass ratio of methyl methacrylate, styrene and hexafluorobutyl methacrylate is (3-8):(2-4):(1-3), preferably 5:3:2.
[0014] The preparation method of the alkali-soluble resin is specifically as follows:
[0015] Methyl methacrylate, styrene and hexafluorobutyl methacrylate are dissolved in an organic solvent according to the formula, heated to a reflux temperature of 90-105°C, 2 / 3 of an initiator is added, and the reflux reaction is carried out for 5-8 hours; the remaining initiator is then added, and the reaction is continued for 2-3 hours. After cooling, the reaction mixture is transferred to a distillation device, and the organic solvent is distilled off to obtain the alkali-soluble resin.
[0016] The initiator is benzoyl peroxide BPO or azobisisobutyronitrile AIBN. The content of the initiator is 3%-5% of the total amount of acrylic resin monomers.
[0017] The organic solvent is selected from one of ethanol, butanone and n-butanol. The content of the organic solvent is 50%-80% of the total amount of the acrylic resin monomer.
[0018] The photosensitive monomer is a mixture of propoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and perfluorooctyl ethyl methacrylate.
[0019] Furthermore, the mass ratio of propoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and perfluorooctyl ethyl methacrylate in the photosensitive monomer is (3-8):(3-8):(1-3), preferably 3:4:3.
[0020] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0021] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0022] A second object of the present invention is to provide a method for preparing a photosensitive dry film coating, comprising the following steps:
[0023] (1) Weigh the raw materials of each component according to the formula;
[0024] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 200-300 r / min for 1-2 hours at room temperature to obtain the photosensitive dry film coating.
[0025] The third object of the present invention is to provide a photosensitive dry film, which is obtained by coating or spraying the photosensitive dry film coating on the surface of a polyester PET film and placing it in an oven at a temperature of 70-85°C for drying for 5-10 minutes. The thickness of the photosensitive dry film is 25-50 μm.
[0026] A fourth object of the present invention is to provide an application of a photosensitive dry film coating for improving the resolution and adhesion of a photosensitive dry film.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] (1) The inventors creatively selected an alkali-soluble resin obtained by copolymerizing a plurality of acrylic resin monomers as a film-forming resin for photosensitive dry film coatings, and adjusted the ratio of the soft segment (methyl methacrylate, hexafluorobutyl methacrylate) and the hard segment (styrene) in the acrylic resin by synergistically combining methyl methacrylate, styrene and hexafluorobutyl methacrylate in the acrylic resin monomers, and added hexafluorobutyl methacrylate to improve the resolution and adhesion of the photosensitive dry film.
[0029] (2) The inventors creatively selected a combination of multiple photosensitive monomers, specifically propoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and perfluorooctyl ethyl methacrylate as photosensitive monomers. By adjusting the ratio of the three monomers, propoxy groups and fluorine-containing segments were introduced on the basis of multifunctional acrylates. The three monomers cooperated synergistically to further improve the resolution and adhesion of the photosensitive dry film. DETAILED DESCRIPTION
[0030] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0031] Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art. However, if there is any conflict, the definitions in this specification shall prevail.
[0032] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0033] Preparation of alkali soluble resin JA-1:
[0034] Methyl methacrylate, styrene and hexafluorobutyl methacrylate were dissolved in an organic solvent, butanone, according to the formula, and heated to a reflux temperature of 100° C., and then 2 / 3 of the initiator AIBN was added, and the reaction was refluxed for 8 hours. The remaining initiator AIBN was then added, and the reaction was continued for 3 hours. After cooling, the reaction mixture was transferred to a distillation device, and after distilling out the organic solvent, the alkali-soluble resin JA-1 was obtained.
[0035] Among them, the mass parts of methyl methacrylate, styrene and hexafluorobutyl methacrylate are 40 parts, 30 parts and 30 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts.
[0036] Preparation of alkali soluble resin JA-2:
[0037] Methyl methacrylate, styrene and hexafluorobutyl methacrylate were dissolved in an organic solvent, butanone, according to the formula, and heated to a reflux temperature of 100° C., and then 2 / 3 of the initiator AIBN was added, and the reaction was refluxed for 8 hours. The remaining initiator AIBN was then added, and the reaction was continued for 3 hours. After cooling, the reaction mixture was transferred to a distillation device, and after distilling out the organic solvent, the alkali-soluble resin JA-2 was obtained.
[0038] Among them, the mass parts of methyl methacrylate, styrene and hexafluorobutyl methacrylate are 50 parts, 30 parts and 20 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts.
[0039] Preparation of alkali soluble resin JA-3:
[0040] Methyl methacrylate, styrene and hexafluorobutyl methacrylate were dissolved in an organic solvent, butanone, according to the formula, and heated to a reflux temperature of 100° C., and then 2 / 3 of the initiator AIBN was added, and the reaction was refluxed for 8 hours. The remaining initiator AIBN was then added, and the reaction was continued for 3 hours. After cooling, the reaction mixture was transferred to a distillation device, and after distilling out the organic solvent, the alkali-soluble resin JA-3 was obtained.
[0041] Among them, the mass parts of methyl methacrylate, styrene and hexafluorobutyl methacrylate are 60 parts, 30 parts and 10 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts.
[0042] Preparation of alkali soluble resin JA-4:
[0043] Methyl methacrylate, styrene and hexafluorobutyl methacrylate were dissolved in an organic solvent, butanone, according to the formula, and heated to a reflux temperature of 100° C., and then 2 / 3 of the initiator AIBN was added, and the reaction was refluxed for 8 hours. The remaining initiator AIBN was then added, and the reaction was continued for 3 hours. After cooling, the reaction mixture was transferred to a distillation device, and after distilling out the organic solvent, the alkali-soluble resin JA-4 was obtained.
[0044] Among them, the mass parts of methyl methacrylate, styrene and hexafluorobutyl methacrylate are 40 parts, 40 parts and 20 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts.
[0045] Preparation of alkali soluble resin JC-1:
[0046] Methyl methacrylate and styrene were dissolved in an organic solvent, butanone, according to the formula, and heated to a reflux temperature of 100° C., and then 2 / 3 of the initiator AIBN was added, and the reaction was refluxed for 8 hours. The remaining initiator AIBN was then added, and the reaction was continued for 3 hours. After cooling, the reaction mixture was transferred to a distillation device, and after distilling out the organic solvent, the alkali-soluble resin JC-1 was obtained.
[0047] Among them, the mass parts of methyl methacrylate and styrene are 80 parts and 20 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts.
[0048] Preparation of alkali soluble resin JC-2:
[0049] According to the formula, methyl methacrylate and hexafluorobutyl methacrylate were dissolved in an organic solvent, butanone, and heated to a reflux temperature of 100°C, and then 2 / 3 of the initiator AIBN was added, and the reaction was refluxed for 8 hours. The remaining initiator AIBN was then added, and the reaction was continued for 3 hours. After cooling, the reaction mixture was transferred to a distillation device, and the organic solvent was distilled off to obtain the alkali-soluble resin JC-2.
[0050] Among them, the mass parts of methyl methacrylate and hexafluorobutyl methacrylate are 80 parts and 20 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts.
[0051] Preparation of alkali soluble resin JC-3:
[0052] Dissolve styrene and hexafluorobutyl methacrylate in an organic solvent, butanone, according to the formula, heat to a reflux temperature of 100°C, add 2 / 3 of the initiator AIBN, and reflux for 8 hours. Add the remaining initiator AIBN, continue to react for 3 hours, and after cooling, transfer the reaction mixture to a distillation device. After distilling out the organic solvent, the alkali-soluble resin JC-3 is obtained;
[0053] Among them, the mass parts of styrene and hexafluorobutyl methacrylate are 80 parts and 20 parts respectively; the mass part of initiator AIBN is 5 parts, and the mass part of butanone is 80 parts;
[0054] Photosensitive monomer G-1 G-2 GC-1 GC-2 GC-3 Propoxylated trimethylolpropane triacrylate 30 servings 40 servings 70 servings 70 servings 0 copies Pentaerythritol tetraacrylate 40 servings 40 servings 30 servings 0 copies 70 servings Perfluorooctyl ethyl methacrylate 30 servings 20 servings 0 copies 30 servings 30 servings Example
[0055] A photosensitive dry film coating, comprising the following components in parts by weight:
[0056] Alkali soluble resin JA-1 60 parts
[0057] Photosensitive monomer G-1 30 parts
[0058] Photoinitiator 3 parts
[0059] 10 parts of solvent.
[0060] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0061] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0062] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0063] (1) Weigh the raw materials of each component according to the formula;
[0064] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0065] A photosensitive dry film coating, comprising the following components in parts by weight:
[0066] Alkali soluble resin JA-2 60 parts
[0067] Photosensitive monomer G-1 30 parts
[0068] Photoinitiator 3 parts
[0069] 10 parts of solvent.
[0070] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0071] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0072] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0073] (1) Weigh the raw materials of each component according to the formula;
[0074] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0075] A photosensitive dry film coating, comprising the following components in parts by weight:
[0076] Alkali soluble resin JA-3 60 parts
[0077] Photosensitive monomer G-1 30 parts
[0078] Photoinitiator 3 parts
[0079] 10 parts of solvent.
[0080] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0081] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0082] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0083] (1) Weigh the raw materials of each component according to the formula;
[0084] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0085] A photosensitive dry film coating, comprising the following components in parts by weight:
[0086] Alkali soluble resin JA-4 60 parts
[0087] Photosensitive monomer G-1 30 parts
[0088] Photoinitiator 3 parts
[0089] 10 parts of solvent.
[0090] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0091] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0092] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0093] (1) Weigh the raw materials of each component according to the formula;
[0094] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0095] A photosensitive dry film coating, comprising the following components in parts by weight:
[0096] Alkali soluble resin JA-1 60 parts
[0097] Photosensitive monomer G-2 30 parts
[0098] Photoinitiator 3 parts
[0099] 10 parts of solvent.
[0100] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0101] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0102] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0103] (1) Weigh the raw materials of each component according to the formula;
[0104] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0105] A photosensitive dry film coating, comprising the following components in parts by weight:
[0106] Alkali soluble resin JA-2 60 parts
[0107] Photosensitive monomer G-2 30 parts
[0108] Photoinitiator 3 parts
[0109] 10 parts of solvent.
[0110] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0111] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0112] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0113] (1) Weigh the raw materials of each component according to the formula;
[0114] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0115] A photosensitive dry film coating, comprising the following components in parts by weight:
[0116] Alkali soluble resin JA-2 65 parts
[0117] Photosensitive monomer G-1 25 parts
[0118] Photoinitiator 3 parts
[0119] 10 parts of solvent.
[0120] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0121] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0122] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0123] (1) Weigh the raw materials of each component according to the formula;
[0124] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating. Example
[0125] A photosensitive dry film coating, comprising the following components in parts by weight:
[0126] Alkali soluble resin JA-2 55 parts
[0127] Photosensitive monomer G-1 35 parts
[0128] Photoinitiator 3 parts
[0129] 10 parts of solvent.
[0130] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0131] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0132] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0133] (1) Weigh the raw materials of each component according to the formula;
[0134] (2) adding an alkali-soluble resin, a photosensitive monomer, a photoinitiator and a solvent into a stirring kettle in sequence, and stirring at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating;
[0135] A photosensitive dry film coating, comprising the following components in parts by weight:
[0136] Alkali soluble resin JC-1 60 parts
[0137] Photosensitive monomer G-1 30 parts
[0138] Photoinitiator 3 parts
[0139] 10 parts of solvent.
[0140] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0141] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0142] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0143] (1) Weigh the raw materials of each component according to the formula;
[0144] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0145] A photosensitive dry film coating, comprising the following components in parts by weight:
[0146] Alkali soluble resin JC-2 60 parts
[0147] Photosensitive monomer G-1 30 parts
[0148] Photoinitiator 3 parts
[0149] 10 parts of solvent.
[0150] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0151] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0152] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0153] (1) Weigh the raw materials of each component according to the formula;
[0154] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0155] A photosensitive dry film coating, comprising the following components in parts by weight:
[0156] Alkali soluble resin JC-3 60 parts
[0157] Photosensitive monomer G-1 30 parts
[0158] Photoinitiator 3 parts
[0159] 10 parts of solvent.
[0160] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0161] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0162] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0163] (1) Weigh the raw materials of each component according to the formula;
[0164] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0165] A photosensitive dry film coating, comprising the following components in parts by weight:
[0166] Alkali soluble resin JA-2 60 parts
[0167] Photosensitive monomer GC-1 30 parts
[0168] Photoinitiator 3 parts
[0169] 10 parts of solvent.
[0170] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0171] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0172] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0173] (1) Weigh the raw materials of each component according to the formula;
[0174] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0175] A photosensitive dry film coating, comprising the following components in parts by weight:
[0176] Alkali soluble resin JA-2 60 parts
[0177] Photosensitive monomer GC-2 30 parts
[0178] Photoinitiator 3 parts
[0179] 10 parts of solvent.
[0180] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0181] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0182] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0183] (1) Weigh the raw materials of each component according to the formula;
[0184] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0185] A photosensitive dry film coating, comprising the following components in parts by weight:
[0186] Alkali soluble resin JA-2 60 parts
[0187] Photosensitive monomer GC-3 30 copies
[0188] Photoinitiator 3 parts
[0189] 10 parts of solvent.
[0190] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0191] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0192] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0193] (1) Weigh the raw materials of each component according to the formula;
[0194] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0195] A photosensitive dry film coating, comprising the following components in parts by weight:
[0196] Alkali soluble resin JC-1 60 parts
[0197] Photosensitive monomer GC-1 30 parts
[0198] Photoinitiator 3 parts
[0199] 10 parts of solvent.
[0200] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0201] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0202] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0203] (1) Weigh the raw materials of each component according to the formula;
[0204] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0205] A photosensitive dry film coating, comprising the following components in parts by weight:
[0206] Alkali soluble resin JC-2 60 parts
[0207] Photosensitive monomer GC-2 30 parts
[0208] Photoinitiator 3 parts
[0209] 10 parts of solvent.
[0210] The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1.
[0211] The solvent is a mixture of acetone and toluene in a mass ratio of 1:2.
[0212] The method for preparing the above-mentioned photosensitive dry film comprises the following steps:
[0213] (1) Weigh the raw materials of each component according to the formula;
[0214] (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 300 r / min for 2 h at room temperature to obtain the photosensitive dry film coating.
[0215] Photosensitive dry film sample preparation:
[0216] The photosensitive dry film coatings of Examples 1-8 and Comparative Examples 1-8 were coated on the surface of the polyester PET film, placed in an oven at a temperature of 85° C. and dried for 10 minutes to obtain a photosensitive dry film, the thickness of the photosensitive dry film being 25 μm.
[0217] Photosensitive dry film performance test:
[0218] (1) Pretreatment: Use a volcanic ash grinding machine to pre-treat the copper clad laminate;
[0219] (2) Film lamination: Use a manual film laminating machine for film lamination at a temperature of 100°C and a film laminating speed of 1.5 m / s.
[0220] (3) Exposure: The exposure source is a 5 kW high-pressure mercury lamp with a wavelength of 365 nm and an exposure energy of 60 mJ / cm 2 .
[0221] (4) Development: Using 1.0% Na 2 CO3 aqueous solution was used as the developer, the developing temperature was 30°C, and the pressure was 2.0 kg / cm 2 , development time 45s.
[0222] (5) De-filming: Use a strong alkali to saponify and dissolve the solidified material. Use a 5% sodium hydroxide aqueous solution. The de-filming temperature is 50°C and the de-filming pressure is 2.0 kg / cm 2 .
[0223] Resolution and adhesion test:
[0224] Resolution test: Use RP-1 test pattern (L / S=1 / 1);
[0225] Adhesion test adopts the grid method: use a blade with a blade distance of 5mm (blade angle of 20°±5°) to scratch 10×10 grids of 10mm×10mm on the surface of the photosensitive dry film, and use tape to stick and cover all the grids on each test block. The tape cannot be wrinkled and is rubbed hard with an eraser to increase the contact area and strength between the tape and the grids. Quickly tear off the tape and record the number of grids adhered to the tape. The more grids adhered, the worse the adhesion.
[0226] The performance results are shown in Table 1-Table 2;
[0227] Table 1
[0228] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Resolution / μm 22 20 25 23 23 21 23 22 Adhesion / grid number 2 0 3 3 2 1 3 2
[0229] Table 2
[0230] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Resolution / μm 38 35 37 40 37 41 45 43 Adhesion / grid number 20 32 25 25 31 23 42 45
[0231] By comparing Examples 1-8 in Table 1 with Comparative Examples 1-8 in Table 2, it can be seen that the photosensitive dry film coating of the present invention produces a synergistic effect between the monomers in the alkali-soluble resin, a synergistic effect between the raw materials of the photosensitive monomer, and a synergistic effect between the alkali-soluble resin and the photosensitive monomer by adjusting the ratio of methyl methacrylate, styrene and hexafluorobutyl methacrylate in the alkali-soluble resin, and the ratio of propoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and perfluorooctylethyl methacrylate in the photosensitive monomer. The comprehensive effect makes the obtained photosensitive dry film have good resolution and adhesion, among which the various properties of Example 2 are the best.
[0232] By comparing Examples 1-8 in Table 1 with Comparative Examples 7-8 in Table 2, it can be seen that when the alkali-soluble resin and the photosensitive monomer are not made of the raw materials protected by the present application, the adhesion and resolution are poor.
[0233] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the embodiments of the present invention rather than to limit them. Although the embodiments of the present invention have been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the embodiments of the present invention can still be modified or replaced by equivalents, and these modifications or equivalent replacements cannot cause the modified technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A photosensitive dry film coating, It is characterized in that According to weight parts, it is composed of the following raw materials: 40-70 parts of alkali soluble resin Photosensitive monomer 20-50 parts Photoinitiator 0.05-5 parts 10-20 parts of solvent; The alkali-soluble resin is an acrylic resin, specifically a copolymer obtained by polymerizing the following acrylic resin monomers: methyl methacrylate, styrene and hexafluorobutyl methacrylate; The mass ratio of methyl methacrylate, styrene and hexafluorobutyl methacrylate is (3-8): (2-4): (1-3); The photosensitive monomer is a mixture of propoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and perfluorooctyl ethyl methacrylate; The mass ratio of propoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and perfluorooctyl ethyl methacrylate in the photosensitive monomer is (3-8): (3-8): (1-3); The photoinitiator is a mixed photoinitiator of o-chlorohexaarylbisimidazole BCIM and tetraethyl Michler's ketone EMK in a mass ratio of 10:1; The solvent is a mixture of acetone and toluene in a mass ratio of 1:
2.
2. The photosensitive dry film coating according to claim 1, It is characterized in that The preparation method of the alkali-soluble resin is specifically as follows: Dissolve methyl methacrylate, styrene and hexafluorobutyl methacrylate in an organic solvent according to the formula, heat to a reflux temperature of 90-105°C, add 2 / 3 of the initiator, reflux for 5-8 hours, then add the remaining initiator, continue to react for 2-3 hours, transfer the reaction mixture to a distillation device after cooling, and distill off the organic solvent to obtain the alkali-soluble resin; The initiator is benzoyl peroxide BPO or azobisisobutyronitrile AIBN, and the content of the initiator is 3%-5% of the total amount of acrylic resin monomer; The organic solvent is selected from one of ethanol, butanone and n-butanol, and the content of the organic solvent is 50%-80% of the total amount of the acrylic resin monomer.
3. A method for preparing the photosensitive dry film coating according to any one of claims 1 to 2, It is characterized in that The steps include: (1) Weigh the raw materials of each component according to the formula of claim 1; (2) Alkali-soluble resin, photosensitive monomer, photoinitiator and solvent are added into a stirring kettle in sequence, and stirred at a speed of 200-300 r / min for 1-2 hours at room temperature to obtain the photosensitive dry film coating.
4. A photosensitive dry film, It is characterized in that The photosensitive dry film coating according to any one of claims 1 to 2 or the photosensitive dry film coating prepared according to claim 3 is coated or sprayed on the surface of a polyester PET film, and placed in an oven at a temperature of 70-85° C. to dry for 5-10 minutes to obtain the photosensitive dry film.
5. A photosensitive dry film according to claim 4, It is characterized in that The photosensitive dry film has a thickness of 25-50 μm.
6. Use of the photosensitive dry film coating according to any one of claims 1 to 2 or the photosensitive dry film coating prepared according to claim 3 to improve the resolution and adhesion of a photosensitive dry film.
Citation Information
Patent Citations
Composition and organic thin-film transistor using same
CN106062935A
Ultraviolet light polymerization super-hydrophobic transparent wear-resistant coating and preparation method thereof
CN107254207A
Fluorine-containing photosensitive resin for black matrix photoresist and resin composition of fluorine-containing photosensitive resin
CN111574656A
Preparation method of photoresist film-forming resin and photoresist composition thereof
CN112679653A
Alkali-soluble resin as well as composition and application thereof
CN115586702A