Preparation method and application of hydroxychlorocopper hydrotalcite composite catalyst
By controlling the distribution pH of the copper hydroxyl chloride hydrotalcite composite catalyst by the single drop method and the microwave hydrothermal crystallization method, the problems of insufficient stability and mineralization ability of the existing copper-based hydrotalcite and copper hydroxyl chloride catalysts in wastewater treatment are solved. , achieving efficient mineralization of organic compounds containing aromatic rings and rapid regeneration of catalysts.
Patent Information
- Application Number
- CN202410144323.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-02-01
AI Technical Summary
Existing copper-based hydrotalcite and copper hydroxychloride catalysts have problems in wastewater treatment, such as difficulty in rapid regeneration, poor stability, long synthesis time, and high energy consumption, especially when dealing with other aromatic ring-containing organic matter. The mineralization ability is insufficient.
A hydroxyl-copper chloride hydrotalcite composite catalyst is used, which is composed of copper-based hydrotalcite and copper hydroxyl chloride grown in situ on the laminate. It is prepared by distributed pH-controlled single drop method and microwave hydrothermal crystallization method to simplify the process and improve the catalyst mineralization properties and stability.
It achieves efficient mineralization of a variety of aromatic ring-containing organic compounds, significantly improves catalyst stability and regeneration performance, shortens synthesis time, reduces energy consumption, uses less catalyst and does not require adjustment of reaction pH, and has a low metal copper dissolution rate.
Smart Images

Figure CN118022781B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wastewater treatment, in particular to a method for preparing a hydroxychlorocopper hydrotalcite composite catalyst and application thereof in organic wastewater degradation. Background Art
[0002] Fenton oxidation technology is a deep oxidation treatment technology that is widely used in this type of wastewater treatment. However, the homogeneous Fe-based catalytic system is limited by the difficulty of catalyst recycling and reuse, the narrow reaction pH range (2-4), and the secondary pollution caused by iron salt sludge. The heterogeneous Fenton catalytic system has largely overcome the shortcomings of the homogeneous system. Copper has a similar redox cycle to Fe in the Fenton reaction. + / Cu 2+ The reaction rate constants with H2O2 are much greater than those with Fe 2+ / Fe 3+ , showing higher oxidative degradation efficiency, and its applicable pH range is wider, and it can be used in a near-neutral environment. Therefore, Cu-based heterogeneous Fenton catalysts are of great application value.
[0003] Hydrotalcite is a layered clay material with a host-guest structure. Its preparation method is simple, its structural composition can be adjusted flexibly, and its special layer structure can achieve high dispersion of active metals. Therefore, it is of great value to introduce active metal Cu into the hydrotalcite layer to prepare hydrotalcite materials and apply them to wastewater treatment. The patents CN107398277A and CN111054358B applied by the inventor previously disclosed the preparation and application of CuNiFe and CuNiSn ternary copper-containing hydrotalcites, respectively, and pointed out that the advantages of this type of catalyst are Cu + Through the Ni 2+ The electron transfer between CuNiSn and CuNiSn can achieve rapid regeneration, especially the closed electron cycle in CuNiSn hydrotalcite, which can further promote the + Rapid regeneration; in addition, hydrotalcite also has good catalytic stability. However, the above patent only proves the catalytic mineralization effect of copper-containing hydrotalcite on phenol, but its mineralization ability for other aromatic ring-containing organic matter still needs to be further improved. In addition, the synthesis of the catalyst requires long-term hydrothermal crystallization of 10 to 24 hours, which is time-consuming and energy-intensive.
[0004] Hydroxycopper chloride is a layered copper mineral, mainly composed of copper hydroxyl octahedrons and copper octahedron units in which some hydroxyl groups are replaced by chlorine. The inventor's previously disclosed patent CN112916025B reported a hydroxycopper chloride catalyst, preparation method and application. Hydroxycopper chloride was synthesized by coprecipitation and used as a Fenton catalyst to mineralize organic pollutants such as phenol, salicylic acid, 2-chlorophenol, bisphenol A, and benzoic acid. The catalyst can achieve faster Cu+ / Cu 2+ The catalyst can efficiently degrade and mineralize organic pollutants due to the high HO· cycle and higher HO· production. However, a certain amount of copper ions are dissolved in the solution, and the catalytic stability needs to be improved. In addition, the synthesis of the catalyst requires long-term hydrothermal crystallization of 16 to 24 hours, which is time-consuming and energy-intensive. Summary of the invention
[0005] In view of the above-mentioned deficiencies of existing copper-based hydrotalcite and hydroxycopper chloride, the present invention prepares a hydroxycopper chloride hydrotalcite composite catalyst. The composite catalyst is composed of copper-based hydrotalcite and hydroxycopper chloride grown in situ on its layer plate. The composite catalyst makes up for the defects of copper-based hydrotalcite and hydroxycopper chloride respectively, and can also produce a synergistic effect to further improve the mineralization performance and stability of the catalyst. Moreover, the preparation method of the catalyst is also characterized by simple process and short time consumption.
[0006] The preparation method of the hydroxychlorocopper hydrotalcite composite catalyst provided by the present invention is as follows:
[0007] S1: Dissolve soluble copper salt, nickel salt and aluminum salt in boiled deionized water to obtain mixed salt solution A; dissolve NaOH in boiled deionized water to obtain alkaline solution B. In solution A, the molar ratio of Cu to Ni is 1 to 4, and the molar ratio of the total number of Cu and Ni to the molar number of Al is 1 to 3.
[0008] S2: adopting the step-by-step pH control single drop method: stirring solution A at a rotation speed of 1000 rpm at room temperature, adding solution B dropwise into solution A during stirring, stopping adding solution B when the pH of solution A rises to 4.5-5.5, stirring and reacting for 10-30 minutes, and then continuing to drop solution B until the pH of solution A rises to 6.5-9.0, stopping adding solution B, completing the addition, and continuing to stir and react at 20-50°C for 10-30 minutes to obtain slurry C.
[0009] S3: placing the slurry C in a microwave reactor, hydrothermally crystallizing it at 80-120° C. for 20-40 min, and then filtering, washing and drying to obtain a hydroxychlorocopper hydrotalcite composite catalyst.
[0010] Preferably, in step S1, Cu in solution A 2+ The concentration is 0.05-0.10 mol / L, the soluble copper salt is selected from copper chloride; the soluble nickel salt is selected from nickel chloride or nickel nitrate; the soluble aluminum salt is selected from aluminum chloride or aluminum nitrate.
[0011] Preferably, the concentration of NaOH in the alkaline solution B is 0.1 to 0.5 mol / L.
[0012] Preferably, in step S2, the dropping speed of solution B is 0.75-1.0 mL / min.
[0013] The catalyst is used to degrade organic wastewater containing aromatic rings. Specific application method: When the catalyst degrades organic wastewater containing aromatic rings, the catalyst addition amount is 0.1-0.4 g / L, the H2O2 concentration is 18-53 mmol / L, the reaction temperature is 30-50°C, and the reaction time is 0.5-3 hours.
[0014] Compared with the prior art, the present invention is beneficial in that:
[0015] (1) The preparation method of the hydroxychlorocopper hydrotalcite composite of the present invention adopts a distributed pH-controlled single-drop method that can control the precipitation reaction of copper ions, overcoming the conventional double-drop method, which is easy to form a single hydrotalcite phase during the co-precipitation of multiple metal ions and is difficult to form a hydroxychlorocopper hydrotalcite composite; and microwave hydrothermal crystallization can shorten the synthesis time of the composite from more than 12 hours of traditional hydrothermal crystallization to less than 40 minutes, and has a higher crystallinity. The method is simple, time-saving, does not require high-temperature roasting, and the raw materials are cheap and easy to obtain.
[0016] (2) The hydroxychlorocopper hydrotalcite complex prepared by the present invention has excellent mineralization performance for various aromatic ring-containing organic matter in wastewater as a Fenton catalyst, and the amount of catalyst used is small, and there is no need to adjust the pH value of the reaction system. The dissolution rate of metallic copper is low and the catalyst stability is good.
[0017] (3) The hydroxycopper chloride-hydrotalcite composite catalyst prepared by the present invention not only makes up for the defects of the single hydroxycopper chloride and hydrotalcite catalysts, but also the synergistic effect of the composite catalytic material can further improve the mineralization performance and stability of the catalyst. The corresponding catalytic activity is significantly better than that of the single hydroxycopper chloride and hydrotalcite catalysts, and the metal dissolution is less and the catalyst stability is better.
[0018] (4) The hydroxychlorocopper hydrotalcite composite catalyst prepared by the present invention has an in-situ formation of the hydroxychlorocopper structure, which aggravates the distortion of the hydrotalcite layer, resulting in a large number of oxygen vacancies in the structure, thereby promoting the generation of superoxide free radicals, so that hydroxyl free radicals and superoxide free radicals exist in the system as oxidizing species at the same time, significantly improving the catalytic mineralization ability and Cu + The regeneration speed is very fast and has great potential in treating industrial wastewater.
[0019] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1The XRD diagrams are of the hydroxycopper chloride (a) and hydrotalcite (b) prepared in Comparative Examples 1 and 2 and the hydroxycopper chloride hydrotalcite composite (c) prepared in Example 1.
[0021] Figure 2 The XRD spectra of samples obtained by different feeding methods or crystallization methods, wherein (a) represents the sample prepared in Comparative Example 3, (b) represents the sample prepared in Comparative Example 4, (c) represents the sample prepared in Comparative Example 5, and (d) represents the sample prepared in Example 1. DETAILED DESCRIPTION
[0022] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0023] In the following examples, Cu / Ni refers to the molar ratio of Cu element to Ni element. (Cu+Ni) / Al refers to the ratio of the total molar number of Cu element in soluble copper salt and Ni element in soluble nickel salt to the total molar number of Al element in soluble aluminum salt.
[0024] Example 1
[0025] A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst comprises the following steps:
[0026] Weigh copper chloride, nickel nitrate and aluminum nitrate separately and dissolve them in boiled deionized water to prepare Cu 2+ A mixed salt solution A with a concentration of 0.05 mol / L, Cu / Ni=3, (Cu+Ni) / Al=2; sodium hydroxide is weighed and dissolved in boiled deionized water to prepare an alkaline solution B with a molar concentration of 0.3 mol / L. Under room temperature and vigorous stirring (speed 1000 rpm) of solution A, solution B is slowly added dropwise (drop speed 1.0 mL / min) until the pH of solution A rises to 4.5, the dropwise addition of solution B is suspended, and after stirring for 10 minutes, solution B is continued to be added dropwise at the same dropwise rate until the end point pH=8.0. After the addition is completed, the stirring reaction is continued at 20°C for 30 minutes to obtain slurry C. Slurry C is transferred to a microwave reactor, hydrothermally crystallized at 100°C in a microwave tester for 30 minutes, and then filtered and washed until the filtrate is neutral, and the product is dried at 80°C for 6 hours to obtain a hydroxychlorocopper hydrotalcite composite catalyst.
[0027] Example 2
[0028] A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst. The preparation steps of this embodiment are the same as those of embodiment 1, except that in the mixed salt solution A, Cu / Ni=1, (Cu+Ni) / Al=2, and the concentration of sodium hydroxide is 0.1 mol / L; the pH value of the end point of the dropwise addition of solution B=6.5, and the stirring reaction is continued at 35° C. for 30 min after the addition is completed; and the crystallization process is microwave hydrothermal crystallization at 80° C. for 40 min.
[0029] Example 3
[0030] A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst. The operating steps of this embodiment are the same as those of embodiment 1, except that in the mixed salt solution A, Cu / Ni=2, (Cu+Ni) / Al=1.5; the pH of the solution A is 5.0 during the intermediate pause stage of dripping the solution B, and the pH at the end point of dripping the solution B is 8.0; and the crystallization process is microwave hydrothermal crystallization at 80°C for 30 minutes.
[0031] Example 4
[0032] A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst. The operating steps of this embodiment are the same as those of embodiment 1, except that in the mixed salt solution A, Cu / Ni=2, (Cu+Ni) / Al=3, and the concentration of sodium hydroxide is 0.5 mol / L; the pH of the solution in the intermediate pause stage of dripping solution B=5.5, the pH at the end point of dripping solution B=9.0, and then stirring is continued at 50°C for 30 minutes to fully react; and the crystallization process is microwave hydrothermal crystallization at 120°C for 20 minutes.
[0033] Example 5
[0034] A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst. The operating steps of this embodiment are the same as those of embodiment 1, except that in the mixed salt solution A, Cu / Ni=2, (Cu+Ni) / Al=2; the endpoint pH of the dropwise addition solution B=7.0; and the crystallization process is microwave hydrothermal crystallization at 100°C for 20 minutes.
[0035] Example 6
[0036] A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst. The operating steps of this embodiment are the same as those of embodiment 1, except that in the mixed salt A solution, Cu / Ni=3, (Cu+Ni) / Al=1.5; the pH of solution A is 5.0 during the intermediate pause stage of dripping solution B, and the pH of solution A is 8.0 at the end point of dripping solution B.
[0037] The preparation conditions and parameters of the hydroxychlorocopper hydrotalcite composites of the above examples are shown in Table 1.
[0038] Table 1. Preparation conditions of hydroxychlorocopper hydrotalcite composites of Examples 1 to 6
[0039]
[0040]
[0041] Comparative Example 1
[0042] A method for preparing hydroxycopper chloride comprises the following steps:
[0043] Weigh copper chloride and dissolve it in boiled deionized water to prepare a 0.5 mol / L copper chloride solution; weigh sodium hydroxide and dissolve it in boiled deionized water to prepare a 0.75 mol / L sodium hydroxide solution. At room temperature and vigorous stirring (speed 1000 rpm), slowly add the copper chloride solution and sodium hydroxide solution (dropping speed 1.0 mL / min) to a flask containing 10 mL of boiled deionized water, and always control the system pH = 7.0. After the addition is completed, continue to stir and react at 20°C for 30 minutes to obtain a slurry. Transfer the slurry into a reactor, hydrothermally crystallize it in an oven at 80°C for 18 hours, then filter, wash, and dry at room temperature to obtain hydroxychlorocopper.
[0044] Comparative Example 2
[0045] A method for preparing copper-nickel-aluminum hydrotalcite comprises the following steps:
[0046] First, copper nitrate, nickel nitrate and aluminum nitrate were weighed and dissolved in boiled deionized water to prepare a mixed salt solution with a copper molar concentration of 0.05 mol / L, Cu / Ni=3, (Cu+Ni) / Al=2; sodium hydroxide was weighed and dissolved in boiled deionized water to prepare an alkaline solution with a molar concentration of 0.3 mol / L. Secondly, under vigorous stirring conditions, the above two solutions were slowly added to a flask containing 10 mL of boiled deionized water at the same time, and the pH of the system was always controlled to be close to 8.0. After the addition was completed, the stirring reaction was continued at 20°C for 30 minutes to obtain a slurry. Finally, the slurry was transferred to a reactor, hydrothermally crystallized at 100°C in an oven for 18 hours, then filtered and washed until the filtrate was neutral, and the product was dried at 80°C for 6 hours to obtain copper-nickel-aluminum hydrotalcite.
[0047] Comparative Example 3
[0048] A preparation method of a hydroxychlorocopper hydrotalcite composite comprises the following steps: copper chloride, nickel nitrate and aluminum nitrate are weighed and dissolved in boiled deionized water to prepare a mixed salt solution A with a copper molar concentration of 0.05 mol / L, Cu / Ni=3, (Cu+Ni) / Al=2; sodium hydroxide is weighed and dissolved in boiled deionized water to prepare an alkaline solution B with a molar concentration of 0.3 mol / L. The amounts of solution A and solution B are the same as those of solution A and solution B in Example 1. At room temperature and under vigorous stirring (rotating speed 1000 rpm), the measured solution A and solution B are simultaneously slowly dripped (drip speed 1.0 mL / min) into a flask containing 10 mL of boiled deionized water, and the pH of the system is always controlled to be about 8.0 during the dripping process. After the addition is completed, the stirring reaction is continued at 20°C for 30 minutes to obtain a slurry C. The slurry C was transferred into a microwave reactor and subjected to microwave hydrothermal crystallization at 100° C. for 30 min in a microwave tester. The slurry was then filtered and washed until the filtrate was neutral. The product was dried at 80° C. for 6 h.
[0049] Comparative Example 4
[0050] A method for preparing a hydroxychlorocopper hydrotalcite composite comprises the following steps:
[0051] Copper chloride, nickel nitrate and aluminum nitrate were weighed and dissolved in boiled deionized water to prepare a mixed salt solution A with a copper molar concentration of 0.05 mol / L, Cu / Ni=3, (Cu+Ni) / Al=2; sodium hydroxide was weighed and dissolved in boiled deionized water to prepare an alkaline solution B with a molar concentration of 0.3 mol / L. Under room temperature and vigorous stirring (speed 1000 rpm) of solution A, solution B was slowly added dropwise (drop speed 1.0 mL / min) until the pH of solution A rose to 4.5, the dropwise addition of solution B was stopped, stirred for 10 minutes, and then solution B was continued to be added dropwise at the same dropwise rate until the end point pH=8.0. After the addition was completed, the stirring reaction was continued at 20°C for 30 minutes to obtain slurry C. Slurry C was hydrothermally crystallized in an oven at 100°C for 18 hours, then filtered and washed until the filtrate was neutral, and the product was dried at 80°C for 6 hours.
[0052] Comparative Example 5
[0053] A method for preparing a hydroxychlorocopper hydrotalcite composite comprises the following steps:
[0054] Copper chloride, nickel nitrate and aluminum nitrate were weighed and dissolved in boiled deionized water to prepare a mixed salt solution A with a copper molar concentration of 0.05 mol / L, Cu / Ni=3, (Cu+Ni) / Al=2; sodium hydroxide was weighed and dissolved in boiled deionized water to prepare an alkaline solution B with a molar concentration of 0.3 mol / L. Under room temperature and vigorous stirring (speed 1000 rpm) of solution A, solution B was slowly added dropwise (dropping speed 1.0 mL / min) until the end point pH=8.0. After the addition was completed, the reaction was continued to stir at 20°C for 30 minutes to obtain slurry C. Slurry C was transferred to a microwave reactor and subjected to microwave hydrothermal crystallization at 100°C for 30 minutes in a microwave tester, then filtered and washed until the filtrate was neutral, and the product was dried at 80°C for 6 hours.
[0055] The XRD spectra of the hydroxycopper chloride prepared in Comparative Example 1, the hydrotalcite prepared in Comparative Example 2 and the hydroxycopper chloride hydrotalcite composite prepared in Example 1 are shown in FIG. Figure 1 , wherein (a) represents hydroxycopper chloride, (b) represents hydrotalcite, and (c) represents the hydroxycopper chloride hydrotalcite composite prepared in Example 1. Figure 1 It can be seen that the hydroxycopper chlorohydroxide composite obtained in Example 1 exhibits an obvious two-phase composite structure of hydroxycopper chlorohydroxide and hydrotalcite, thereby proving that the product prepared in Example 1 is a hydroxycopper chlorohydroxide composite.
[0056] Figure 2 The XRD spectra of samples obtained by different feeding methods or crystallization methods are shown in Figure 1, where (a) represents the sample obtained in Comparative Example 3, (b) represents the sample obtained in Comparative Example 4, (c) represents the sample obtained in Comparative Example 5, and (d) represents the sample obtained in Example 1. Figure 2 It can be seen that compared with Example 1, in Comparative Example 3, other conditions are kept the same, but the sample prepared by the double drop method only shows a single hydrotalcite structure, and a hydroxyl-copper-chloro-hydrotalcite complex cannot be prepared; in Comparative Example 4, other conditions are kept the same, and although a hydroxyl-copper-chloro-hydrotalcite complex is synthesized by conventional hydrothermal crystallization for 18 hours, its crystallinity is much lower than that of the complex sample obtained by microwave hydrothermal crystallization in Example 1, which is only 45% of the latter, and the latter only needs 30 minutes of crystallization time, greatly improving the synthesis efficiency and greatly reducing the energy consumption, which proves the advantage of the microwave hydrothermal crystallization method. In Comparative Example 5, other conditions are kept the same, and although a hydroxyl-copper-chloro-hydrotalcite complex can be synthesized by conventional single drop method, the diffraction peak of the hydroxyl-copper-chloro phase is weak, and its content is too low, indicating that less hydroxyl-copper-chloro is formed during the synthesis process, which further proves the advantage of the distributed pH control single drop method used in the present invention in controlling the copper ion precipitation reaction to form in-situ grown hydroxyl-copper-chloro.
[0057] Fenton catalytic performance test:
[0058] The hydroxycopper chloride hydrotalcite complex prepared in the above examples was used for the Fenton reaction to mineralize aromatic ring-containing organic pollutants, including aniline, phenol, dibutyl phthalate, p-nitrophenol, p-chlorophenol, o-toluidine, and m-cresol, and was compared with single hydroxycopper chloride and copper-nickel-aluminum hydrotalcite catalysts prepared in Comparative Examples 1 and 2.
[0059] Test Example 1:
[0060] The concentration of the aniline aqueous solution was 100 mg / L, the original pH was 7.2, the hydroxychlorocopper prepared in Comparative Example 1 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0061] Test Example 2:
[0062] The concentration of the aniline aqueous solution was 100 mg / L, the original pH was 7.2, the copper-nickel-aluminum hydrotalcite prepared in Comparative Example 2 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0063] Test Example 3:
[0064] The concentration of the aniline aqueous solution was 100 mg / L, the original pH was 7.2, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0065] Test Example 4:
[0066] The concentration of the phenol aqueous solution was 100 mg / L, the original pH was 6.4, the hydroxychlorocopper hydrotalcite complex prepared in Example 3 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0067] Test Example 5:
[0068] The concentration of dibutyl phthalate aqueous solution was 40 mg / L, the original pH was 7.0, the hydroxychlorocopper hydrotalcite complex prepared in Example 6 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 53 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0069] Test Example 6:
[0070] The concentration of the p-nitrophenol aqueous solution was 50 mg / L, the original pH was 6.8, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was determined by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0071] Test Example 7:
[0072] The concentration of the p-chlorophenol aqueous solution was 40 mg / L, the original pH was 7.1, the hydroxychlorocopper hydrotalcite complex prepared in Example 3 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 27 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0073] Test Example 8:
[0074] The concentration of o-toluidine aqueous solution was 50 mg / L, the original pH was 7.5, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.5 g / L, the amount of H2O2 was 53 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0075] Test Example 9:
[0076] The concentration of the m-cresol aqueous solution was 50 mg / L, the original pH was 7.0, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was determined by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0077] Test Example 10:
[0078] The concentration of the aniline aqueous solution was 100 mg / L, the original pH was 7.2, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.2 g / L, the amount of H2O2 was 35 mmol / L, the reaction was stirred at 40°C for 2.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0079] Test Example 11:
[0080] The concentration of the aniline aqueous solution was 100 mg / L, the original pH was 7.2, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.4 g / L, the amount of H2O2 was 27 mmol / L, the reaction was stirred at 40°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0081] Test Example 12:
[0082] The concentration of the aniline aqueous solution was 100 mg / L, the original pH was 7.2, the hydroxychlorocopper hydrotalcite complex prepared in Example 1 was used as a catalyst, the addition amount was 0.2 g / L, the amount of H2O2 was 27 mmol / L, the reaction was stirred at 50°C for 1.5 hours, and the catalyst was removed by filtration after the reaction was completed. The total organic carbon (TOC) value of the wastewater before and after the reaction was measured by a total organic carbon analyzer for calculating the mineralization rate to characterize the Fenton catalytic performance of the material. The calculated mineralization rate is shown in Table 2.
[0083] Table 2. Results of mineralization of pollutants by Fenton reaction using hydroxychlorocopper hydrotalcite composite catalyst
[0084]
[0085] As can be seen from Table 2, the hydroxychlorocopper hydrotalcite composite catalyst of the present invention has a significant mineralization effect on aromatic ring-containing organic matter, and has a mineralization rate of more than 80% for most aromatic ring-containing organic matter, and can mineralize them into non-toxic and harmless carbon dioxide and water, and the reaction conditions are mild, and can achieve effective mineralization of organic matter under the conditions of environmental pH, low H2O2 dosage, and low catalyst dosage. In addition, the catalytic mineralization effect of the composite is significantly better than that of a single hydroxychlorocopper and hydrotalcite catalyst, which confirms that the synergistic effect produced by the two-phase composite catalyst of the present invention can further improve the catalytic mineralization performance of the material.
[0086] Catalyst stability test:
[0087] The stability of the catalyst is tested through a catalyst recycling experiment. The catalyst recycling process is as follows:
[0088] After the above test case experiment is completed, the catalyst in the reaction solution is filtered and recovered, and the mixture is washed alternately three times with boiled deionized water and anhydrous ethanol, and then dried at 80°C for 6 hours to obtain a regenerated catalyst. The same catalytic performance test experiment as the previous test case is repeated using the regenerated catalyst. The recovered and regenerated catalyst is continued to be tested 5 times under the reaction conditions of the original test case. After the fifth cycle, the mineralization rate of the catalyst for organic matter and the copper dissolution value in the solution are shown in Table 3.
[0089] Table 3. Stability test results of hydroxychlorocopper hydrotalcite composite catalyst
[0090]
[0091] It can be seen from Table 3 that the hydroxychlorocopper and hydrotalcite composite catalyst prepared by the present invention has good reproducible and reusable performance. After the catalyst is recycled and regenerated, the organic matter mineralization rate decreases by less than 2% after five reuses, and the copper dissolution value is less than 1 mg / L, which is significantly better than the single hydroxychlorocopper and hydrotalcite catalyst. This shows that the composite catalyst of the present invention has significant stability and practical application value.
[0092] In summary, the preparation method of the hydroxychlorocopper hydrotalcite complex of the present invention has the characteristics of simple preparation procedure, short time consumption, no need for high-temperature calcination, and low raw material cost. At the same time, the complex is used as a Fenton catalyst, which has excellent mineralization performance for various aromatic ring-containing organic matter in wastewater, and the amount of catalyst used is small, there is no need to adjust the pH value of the reaction system, the dissolution rate of metallic copper is low, and the catalyst stability is good.
[0093] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a hydroxychlorocopper hydrotalcite composite catalyst, characterized in that: The catalyst is composed of copper-based hydrotalcite and chlorohydroxy copper in situ grown on its layer plate, and the preparation method has the following steps: S1: dissolving soluble copper salt, nickel salt and aluminum salt in boiled deionized water to obtain a mixed salt solution A; dissolving NaOH in boiled deionized water to obtain an alkaline solution B; wherein the molar ratio of Cu to Ni is 1-4, and the molar ratio of the total number of Cu and Ni to the molar number of Al is 1-3; S2: adopting the step-by-step pH control single drop method: stirring solution A at 1000 rpm at room temperature, adding alkaline solution B to solution A during stirring, stopping the addition of alkaline solution B when the pH of solution A rises to 4.5-5.5, stirring and reacting for 10-30 min, and then continuing to drop alkaline solution B until the pH of solution A rises to 6.5-9.0, stopping the addition of alkaline solution B, completing the addition, and continuing the stirring and reacting at 20-50°C for 10-30 min to obtain slurry C; S3: placing slurry C in a microwave reactor, hydrothermally crystallizing at 80-120° C. for 20-40 min, and then filtering, washing, and drying to obtain a hydroxychlorocopper hydrotalcite composite catalyst.
2. The method for preparing the hydroxychlorocopper hydrotalcite composite catalyst according to claim 1, characterized in that: In step S1, Cu in solution A 2+ The concentration is 0.05~0.10 mol / L.
3. The method for preparing the hydroxychlorocopper hydrotalcite composite catalyst according to claim 1, characterized in that: In step S1, the soluble copper salt is selected from copper chloride; the soluble nickel salt is selected from nickel chloride or nickel nitrate; and the soluble aluminum salt is selected from aluminum chloride or aluminum nitrate.
4. The method for preparing the hydroxychlorocopper hydrotalcite composite catalyst according to claim 1, characterized in that: Step S1, the concentration of NaOH in the alkaline solution B is 0.1-0.5 mol / L.
5. The method for preparing the hydroxychlorocopper hydrotalcite composite catalyst according to claim 1, characterized in that: In step S2, the dropping speed of the alkaline solution B is 0.75-1.0 mL / min.
6. A hydroxychlorocopper hydrotalcite composite catalyst prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the hydroxychlorocopper hydrotalcite composite catalyst as claimed in claim 6, characterized in that: The catalyst is used for degrading organic wastewater containing aromatic rings, wherein pollutants in the organic wastewater contain aniline, phenol, dibutyl phthalate, p-nitrophenol, p-chlorophenol, o-toluidine and m-cresol.
8. The use of the hydroxychlorocopper hydrotalcite composite catalyst as claimed in claim 7, characterized in that: When the catalyst is used to degrade organic wastewater containing aromatic rings, the catalyst addition amount is 0.1-0.4 g / L, the H2O2 concentration is 18-53 mmol / L, the reaction temperature is 30-50°C, and the reaction time is 0.5-3 h.
Citation Information
Patent Citations
Application of Cu-Ni-Fe hydrotalcite-like catalyst in degradation of phenol-containing wastewater
CN107398277A
A copper-nickel-tin hydrotalcite catalyst and its preparation method
CN111054358B
Copper-nickel-tin hydrotalcite catalyst and preparation method thereof
CN111054358A