A novel organosilicon polymer microfluidic chip and its preparation method and application

By adding MVT-PDMS to the PDMS chip, the VPDMS chip is prepared, which solves the problem of lowering the water contact angle after oxygen plasma treatment, realizes efficient droplet generation and simplifies the processing process, and improves the anti-interference ability and production efficiency of the chip.

CN118022869BActive Publication Date: 2024-11-15SHANDONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410293489.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-11-15
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

The existing PDMS microfluidic chips have significantly reduced water contact angle after oxygen plasma treatment, which affects the droplet generation efficiency, and is complex in processing, making it difficult to achieve high productivity and stability.

Method used

Using monovinyl terminated polydimethylsiloxane (MVT-PDMS) to control network expansion, a new silicone polymer (VPDMS) is prepared to maintain high superhydrophobicity after plasma treatment, and to improve the chip's resistance through simplified processes Interference capability.

Benefits of technology

The VPDMS chip maintains a high water contact angle after plasma treatment, which improves droplet generation efficiency and anti-interference ability, shortens processing time, and significantly increases the curing rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118022869B_ABST
    Figure CN118022869B_ABST
Patent Text Reader

Abstract

The present invention relates to a novel organosilicon polymer microfluidic chip, a preparation method and an application thereof. The present invention proposes a strategy of using monovinyl-terminated polydimethylsiloxane (MVT-PDMS) to control network expansion so as to manufacture a novel organosilicon polymer (VPDMS). The addition of MVT-PDMS greatly shortens the processing time of the microfluidic chip. The preparation method is simple, and the generated VPDMS has good resistance to external interference and still has ultra-high hydrophobicity after oxygen plasma treatment. In addition, the novel organosilicon polymer microfluidic chip prepared by the present invention has a shorter curing time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a novel organosilicon polymer microfluidic chip and application thereof. Background Art

[0002] Microfluidics has a wide range of applications in bioinstruments, microsphere manufacturing, and pharmaceuticals. Taking the production of hydrogel microspheres as an example, droplet-based microfluidics usually involves the continuous and stable generation of droplets in the oil and water phases by shearing the water phase with the oil phase. Subsequently, these droplets are solidified into hydrogel microspheres using UV light initiation or other polymerization methods; throughout the process, factors such as the viscosity of the two-phase solution, the flow rate of the two phases, the flow rate ratio, the microfluidic chip structure, the water contact angle in the channel, the temperature and external interference, and the interfacial tension between the two phases play a vital role in the droplet generation process. Therefore, the generation of droplets using microfluidic chips is a complex process that may be interfered by various environmental factors.

[0003] Microfluidic chips are small in size, complex in process, and affected by multiple factors, making it difficult to achieve high productivity and stability in the production process of microfluidic chips. Traditionally, methods to improve droplet yield include modifying the channel structure. For example, adding additional channels for droplet generation or increasing the flow rate and flow rate ratio. However, these methods often require additional energy input and more complex structures. Previous studies have shown that increasing the water contact angle in the channel can improve the efficiency of the oil phase shearing the water phase, thereby increasing the droplet yield. However, improving the water contact angle in the channel usually involves a time-consuming and complex surface modification process, which limits the practical applicability of this method.

[0004] PDMS (polydimethylsiloxane) is often chosen for the manufacture of microfluidic chips due to its high transparency, corrosion resistance, easy preparation, and hydrophobicity. The surfaces of PDMS microfluidic chips and glass substrates are usually modified by plasma treatment to introduce a large number of hydroxyl groups, thereby promoting the formation of Si-O-Si bonds during the bonding process. However, this treatment inevitably leads to a significant decrease in the water contact angle of PDMS, which cannot be restored to its original hydrophobic state. The significant decrease in the water contact angle affects the ability of PDMS microfluidic chips to effectively handle aqueous fluids, thereby reducing the yield of droplets.

[0005] Therefore, how to improve the PDMS chip so that it has a higher ability to resist external interference, that is, it still has ultra-high hydrophobicity after oxygen plasma treatment, is worthy of further study. Summary of the invention

[0006] In view of the shortcomings of the existing chip manufacturing technology, the present invention provides a new type of organosilicon microfluidic chip and its preparation method and application. The present invention proposes a strategy of using monovinyl-terminated polydimethylsiloxane (MVT-PDMS) to control network expansion to manufacture a new organosilicon polymer (VPDMS). The preparation method is simple, and the generated VPDMS has good resistance to external interference. Even after being treated with oxygen plasma (27.6W) for 5 minutes, the VPDMS surface still maintains a high superhydrophobicity (water contact angle: about 171°) during the droplet production process, which is conducive to the generation of droplets.

[0007] The technical solution of the present invention is as follows:

[0008] A novel organosilicon polymer microfluidic chip is a VPDMS chip.

[0009] The method for preparing the novel organosilicon polymer microfluidic chip comprises the following steps:

[0010] (1) Take PDMS, silicone elastomer curing agent and MVT-PDMS, mix them and stir them evenly, and place them in a degasser to remove bubbles;

[0011] (2) Pour the mixed liquid with bubbles removed into the mold, heat it in an oven, and take it out after the chip is solidified;

[0012] (3) Take out the mold and the manufactured chip, demold it, clean the manufactured chip with alcohol, clean the glass slide, and dry them for later use;

[0013] (4) Place the cleaned chip and glass slide into a plasma bonding machine for plasma treatment;

[0014] (5) Quickly attach the processed chip and glass slide and place them in an oven for heating.

[0015] Preferably, according to the present invention, in step (1), the mass ratio of PDMS, silicone elastomer curing agent and MVT-PDMS is 10:1:1 to 10:3:3; preferably, the mass ratio of PDMS, curing agent and MVT-PDMS is 10:2:2.

[0016] Preferably, according to the present invention, in step (1), the weight average molecular weight of the PDMS is 500-100000; preferably, the number average molecular weight of the PDMS is 25000.

[0017] Preferably, according to the present invention, in step (1), the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane; preferably, the viscosity is 40-60 cSt.

[0018] Preferably, according to the present invention, in step (2), the mold is a chip mold printed by a 3D printer.

[0019] Preferably according to the present invention, in step (2), the heating temperature is 50-100°C; preferably, the heating temperature is 60-70°C; the heating time is 20-100 min; preferably, the heating time is 30-40 min.

[0020] Preferably, according to the present invention, in step (4), the treatment time is 3-10 min; preferably, the treatment time is 5 min.

[0021] Preferably according to the present invention, in step (5), the heating temperature is 40-80°C; preferably, the heating temperature is 60°C; the heating time is 5-20 minutes; preferably, the heating time is 10 minutes.

[0022] The present invention also includes the organosilicon polymer microfluidic chip obtained by the above preparation method, and the application of the novel organosilicon polymer microfluidic chip in droplet generation in the pharmaceutical process.

[0023] The technical features and beneficial effects of the present invention are as follows:

[0024] 1. The present invention adopts a simple method to improve the PDMS chip, adding MVT-PDMS to PDMS to reduce the cross-linking density of the PDMS polymer network, so that the polymer network is easy to swell. Due to the sparsity of the polymer network, oil molecules can diffuse more freely between the network and the oil solution to form a stable interfacial oil layer, which effectively isolates the water phase from contact with the hydrophilic functional groups and effectively prevents the water phase from contacting the hydrophilic surface. This phenomenon achieves high superhydrophobicity (water contact angle WCA: 171°) in the channel on a macro scale and exhibits good anti-interference during droplet production.

[0025] 2. The present invention prepares a novel organosilicon polymer microfluidic chip, which is a VPDMS chip. The VPDMS chip exhibits higher initial and final water contact angles than the PDMS chip. The VPDMS chip also has a faster recovery rate after long-term plasma treatment (5min, 27.6 W). The average WCA of the two materials decreased by about 20° after plasma treatment, but the VPDMS chip still maintained a higher WCA than the PDMS chip, which will be more conducive to the generation of droplets.

[0026] 3. The new organosilicon polymer microfluidic chip prepared by the present invention has a shorter curing time. The addition of MVT-PDMS will greatly shorten the processing time of the microfluidic chip. The curing time of the VPDMS chip at 80°C is 122s, and the curing time at 60°C is 814s. For the traditional PDMS chip, the curing time at 80°C is 612s, and no signs of curing are observed at 60°C. Rheological experiments show that the addition of MVT-PDMS increases the curing rate by 502%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the preparation process of VPDMS;

[0028] Figure 2 Schematic diagram of the super-hydrophobic mechanism of the material surface dominated by oil layer in the production environment;

[0029] Figure 3 Comparison of water contact angle (WCA) between plasma-treated and non-plasma-treated VPDMS chips (10:2:2) and PDMS chips;

[0030] Figure 4 Water contact angles of PDMS chip and VPDMS chip (10:2:2) in oil solution after plasma treatment under normal and applied force conditions;

[0031] Figure 5 Schematic diagram of the forces acting on the droplets on the surface of the PDMS chip and the VPDMS chip (10:2:2);

[0032] Figure 6 The friction coefficients of the fresh surface, oiled surface, and deoiled surface of the PDMS chip and the VPDMS chip (10:2:2);

[0033] Figure 7 Storage modulus (G') and loss modulus (G'') of VPDMS chip (10:2:2) and PDMS chip during curing at different temperatures (40℃, 60℃ and 80℃). DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with the accompanying drawings and specific examples, but should not be construed as limiting the present invention. The experimental methods and reagents without specific conditions in the examples are all based on conventional conditions in the art.

[0035] Example 1 A method for preparing a novel organosilicon polymer microfluidic chip

[0036] Here are the steps:

[0037] Step 1, weigh 10g PDMS, 2g silicone elastomer curing agent and 2g MVT-PDMS in a beaker, stir them thoroughly and remove bubbles in a defoamer; the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane with a viscosity of 50cSt.

[0038] Step 2: Pour the solution from which bubbles have been removed into the chip mold printed by the 3D printer. If bubbles are generated during the process of pouring into the mold, the mold should be placed in a debubbler to remove the bubbles. While ensuring that there are no bubbles in the solution in the mold, place the mold in an oven and heat it at 70°C for 30 minutes. After the chip is solidified, take out the mold.

[0039] Step 3: After peeling the chip from the mold, clean the glass slide and the manufactured chip with alcohol to ensure that there is no dust on the surface of the chip and the glass slide.

[0040] Step 4: Place the cleaned chip and glass slide into a plasma bonding machine for surface treatment, and take out the glass slide and chip after 5 minutes.

[0041] Step 5: Quickly attach the removed glass slide and the chip to form a Si-O-Si bond, so that the chip and the glass slide are tightly attached together; then place the glass slide and the chip in an oven and heat them at 60°C for 10 minutes to obtain a new silicone polymer microfluidic chip. Figure 1 shown.

[0042] Example 2 Preparation method of a novel organosilicon polymer microfluidic chip

[0043] Here are the steps:

[0044] Step 1: weigh 10 g of PDMS, 1 g of silicone elastomer curing agent and 2 g of MVT-PDMS in a beaker, stir them thoroughly and remove bubbles in a defoamer; the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane with a viscosity of 50 cSt.

[0045] Step 2: Pour the solution with bubbles removed into the chip mold printed by the 3D printer. If bubbles are generated during the pouring process, the mold should be placed in a debubbler to remove the bubbles. While ensuring that there are no bubbles in the solution, place the mold in an oven and heat it at 60°C for 40 minutes. After the chip is solidified, take out the mold.

[0046] Step 3: After peeling the chip from the mold, clean the glass slide and the manufactured chip with alcohol to ensure that there is no dust on the surface of the chip and the glass slide.

[0047] Step 4: Place the cleaned chip and glass slide into a plasma bonding machine for surface treatment, and take out the glass slide and chip after 7 minutes.

[0048] Step 5: Quickly fit the removed glass slide and chip together to form a Si-O-Si bond, so that the chip and the glass slide fit tightly together; then put the glass slide and chip into an oven and heat them at 50°C for 15 minutes to obtain a new silicone polymer microfluidic chip.

[0049] Example 3 Preparation method of a novel organosilicon polymer microfluidic chip

[0050] Here are the steps:

[0051] Step 1: weigh 10 g of PDMS, 3 g of silicone elastomer curing agent and 2 g of MVT-PDMS in a beaker, stir them thoroughly and remove bubbles in a defoamer; the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane with a viscosity of 50 cSt.

[0052] Step 2: Pour the solution from which bubbles have been removed into the chip mold printed by the 3D printer. If bubbles are generated during the process of pouring into the mold, the mold should be placed in a debubbler to remove the bubbles. While ensuring that there are no bubbles in the solution in the mold, place the mold in an oven and heat it at 50°C for 60 minutes. After the chip is solidified, take out the mold.

[0053] Step 3: After peeling the chip from the mold, clean the glass slide and the manufactured chip with alcohol to ensure that there is no dust on the surface of the chip and the glass slide.

[0054] Step 4: Place the cleaned chip and glass slide into a plasma bonding machine for surface treatment, and take out the glass slide and chip after 4 minutes.

[0055] Step 5: Quickly fit the removed glass slide and chip together to form a Si-O-Si bond, so that the chip and the glass slide fit tightly together; then put the glass slide and chip into an oven and heat them at 60°C for 5 minutes to obtain a new silicone polymer microfluidic chip.

[0056] Example 4 Preparation method of a novel organosilicon polymer microfluidic chip

[0057] Here are the steps:

[0058] Step 1, weigh 10 g PDMS, 2 g silicone elastomer curing agent and 2 g MVT-PDMS in a beaker, stir them thoroughly, and remove bubbles in a defoamer; the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane with a viscosity of 50 cSt.

[0059] Step 2: Pour the solution from which bubbles have been removed into the chip mold printed by the 3D printer. If bubbles are generated during the pouring process, the mold should be placed in a debubbler to remove the bubbles. While ensuring that there are no bubbles in the solution, place the mold in an oven and heat it at 80°C for 20 minutes. After the chip is solidified, take out the mold.

[0060] Step 3: After peeling the chip from the mold, clean the glass slide and the manufactured chip with alcohol to ensure that there is no dust on the surface of the chip and the glass slide.

[0061] Step 4: Place the cleaned chip and glass slide into a plasma bonding machine for surface treatment, and take out the glass slide and chip after 5 minutes.

[0062] Step 5: quickly fit the removed glass slide and chip together to form a Si-O-Si bond, so that the chip and the glass slide fit tightly together; then put the glass slide and the chip into an oven and heat them at 70°C for 10 minutes to obtain a new silicone polymer microfluidic chip.

[0063] Example 5 Preparation method of a novel organosilicon polymer microfluidic chip

[0064] Here are the steps:

[0065] Step 1, weigh 10 g PDMS, 2 g silicone elastomer curing agent and 2 g MVT-PDMS in a beaker, stir them thoroughly, and remove bubbles in a defoamer; the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane with a viscosity of 50 cSt.

[0066] Step 2: Pour the solution from which bubbles have been removed into the chip mold printed by the 3D printer. If bubbles are generated during the process of pouring into the mold, the mold should be placed in a debubbler to remove the bubbles. While ensuring that there are no bubbles in the solution in the mold, place the mold in an oven and heat it at 60°C for 30 minutes. After the chip is solidified, take out the mold.

[0067] Step 3: After peeling the chip from the mold, clean the glass slide and the manufactured chip with alcohol to ensure that there is no dust on the surface of the chip and the glass slide.

[0068] Step 4: Place the cleaned chip and glass slide into a plasma bonding machine for surface treatment, and take out the glass slide and chip after 8 minutes.

[0069] Step 5: Quickly fit the removed glass slide and chip together to form a Si-O-Si bond, so that the chip and the glass slide fit tightly together; then put the glass slide and chip into an oven and heat them at 60°C for 20 minutes to obtain a new silicone polymer microfluidic chip.

[0070] Test example: Performance test of the VPDMS chip obtained by the present invention

[0071] (1) Superhydrophobicity of the surface of the VPDMS chip (10:2:2) obtained in Example 1

[0072] In the experiment, a contact angle goniometer (SDC-200S, Shengding Precision, China) was used to perform contact angle tests, measuring the VPDMS chip (10:2:2) and the PDMS chip before and after plasma treatment.

[0073] The generation of droplets in microfluidic chips involves shearing the water phase from the oil phase. The water contact angles of the VPDMS chip (10:2:2) and the PDMS chip in the production environment are compared. The production environment is a hexadecane solution containing Span 80 (10% by mass). In order to simulate the internal channel environment of the microfluidic chip after bonding, the VPDMS chip (10:2:2) and the PDMS chip were both plasma treated for 5 minutes, as shown in Figure 2. Figure 2 shown.

[0074] The results show that the VPDMS chip (10:2:2) exhibits a higher initial water contact angle than the PDMS chip. The average water contact angles of the two materials decreased by about 20° after plasma treatment, but the VPDMS chip (10:2:2) still maintained a higher water contact angle than the PDMS chip. Figure 3 shown.

[0075] The water contact angle of the VPDMS chip (10:2:2) in the oil phase is as high as 171°, while the water contact angle of the PDMS chip in the oil phase is only 135°. Figure 5 After the disturbance of the droplet and the surface, the droplet quickly broke on the PDMS surface, and the water contact angle of the PDMS chip finally recovered to 43°. The VPDMS chip (10:2:2) still maintained its high superhydrophobicity even after being disturbed, as shown in Figure 4 shown.

[0076] (2) Characterization of the oil layer properties at the interface of the VPDMS chip (10:2:2) obtained in Example 1

[0077] The characterization of the surface oil layer was verified by friction tests, which were performed by a rheometer (MCR 302, Anton Paar). The friction coefficients of the fresh VPDMS chip (10:2:2) and the PDMS chip, the VPDMS chip (10:2:2) and the PDMS chip coated with the oil phase, and the VPDMS chip (10:2:2) and the PDMS chip washed off the oil phase were measured. The steps for applying the oil phase and washing off the oil phase are as follows:

[0078] First, saturate the brush with the oil phase solution and then brush it evenly on the sample surface three times. After that, let the sample stand for 1 minute and then quickly rinse off the oil phase on the sample surface evenly with anhydrous ethanol.

[0079] The presence of oil layers can be quantitatively analyzed by friction analysis. Figure 6 As shown in the figure, with the increase of normal load, the change trend of the friction coefficient of the fresh PDMS surface and the deoiled PDMS surface is similar. Under the load of 5N, the friction coefficient of the deoiled PDMS chip surface is only 4.3% lower than that of the fresh surface. This result shows that hexadecane cannot freely penetrate the polymer network in the PDMS chip, so it cannot form a stable oil layer on the surface. In contrast, the VPDMS chip (10:2:2) sample is able to form a stable oil layer. Even after cleaning with anhydrous ethanol, there are still significant differences in the friction force and friction coefficient between the fresh VPDMS chip surface and the deoiled VPDMS chip surface. Under the load of 5N, the friction coefficient of the deoiled VPDMS chip surface is finally reduced by 28.7% compared with the fresh surface.

[0080] (3) Rheological and mechanical properties of the VPDMS chip (10:2:2) obtained in Example 1

[0081] The mechanical properties of the VPDMS chip (10:2:2) samples were characterized by rheological tests, indentation tests, and adhesion tests.

[0082] like Figure 7 As shown in the figure, the curing time of the VPDMS chip (10:2:2) at 80°C was 122s, the curing time at 60°C was 814s, and there was no sign of curing during the test at 40°C. For the conventional PDMS chip, the curing time at 80°C was 612s, and no sign of curing was observed at 60°C. Rheological experiments showed that the addition of MVT-PDMS increased the curing rate by 502%. The results show that the addition of MVT-PDMS will greatly shorten the processing time of microfluidic chips.

Claims

1. A method for preparing a novel organosilicon polymer microfluidic chip, characterized in that: The method comprises the following steps: (1) Take PDMS, silicone elastomer curing agent and MVT-PDMS, mix them and stir them evenly, and place them in a degasser to remove bubbles; (2) Pour the mixed liquid with bubbles removed into the mold, heat it in an oven, and take it out after the chip is solidified; (3) Take out the mold and the manufactured chip, demold it, clean the manufactured chip with alcohol, clean the glass slide, and dry them for later use; (4) Place the cleaned chip and glass slide into a plasma bonding machine for plasma treatment; (5) Quickly attach the processed chip and glass slide and place them in an oven for heating.

2. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of the PDMS, the silicone elastomer curing agent and the MVT-PDMS is 10:1:1 to 10:3:

3.

3. The preparation method according to claim 2, characterized in that: In step (1), the mass ratio of the PDMS, the curing agent and the MVT-PDMS is 10:2:

2.

4. The preparation method according to claim 1, characterized in that: In step (1), the weight average molecular weight of the PDMS is 500-100000.

5. The preparation method according to claim 4, characterized in that: In step (1), the number average molecular weight of the PDMS is 25,000.

6. The preparation method according to claim 1, characterized in that: In step (1), the MVT-PDMS is α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane.

7. The preparation method according to claim 6, characterized in that: In step (1), the viscosity of the α-monoVINYL-Ω-monoHYDRIDE terminated polydimethylsiloxane is 40-60 cSt.

8. The preparation method according to claim 1, characterized in that: In step (2), the mold is a chip mold printed using a 3D printer.

9. The preparation method according to claim 1, characterized in that: In step (2), the heating temperature is 50-100° C. and the heating time is 20-100 min.

10. The preparation method according to claim 9, characterized in that: In step (2), the heating temperature is 60-70°C and the heating time is 30-40 minutes.

11. The preparation method according to claim 1, characterized in that: In step (4), the treatment time is 3-10 minutes.

12. The preparation method according to claim 11, characterized in that: In step (4), the treatment time is 5 minutes.

13. The preparation method according to claim 1, characterized in that: In step (5), the heating temperature is 40-80° C. and the heating time is 5-20 min.

14. The preparation method according to claim 13, characterized in that: In step (5), the heating temperature is 60° C. and the heating time is 10 min.

15. An organosilicon polymer microfluidic chip obtained by the preparation method according to any one of claims 1 to 14.

16. Use of the novel organosilicon polymer microfluidic chip as claimed in claim 15 in droplet generation in pharmaceutical manufacturing processes.