Root-penetration-resistant double-lapped double-polymer membrane-based waterproofing coiled material and preparation method thereof
By adopting a root puncture-resistant double lapped double polymer membrane-based structure in the waterproof membrane, combined with components such as sodium polyacrylate, manganese dioxide and magnesium silicate, the problem of poor root puncture resistance of the waterproof membrane has been solved, significantly. Improved puncture resistance and root puncture resistance to ensure the waterproof performance of the building.
Patent Information
- Application Number
- CN202410204613.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-02-24
AI Technical Summary
Existing waterproofing membranes have poor resistance to plant root punctures, causing roof leakage and affecting the safety and quality of building structures.
It uses root puncture-resistant double overlapped double polymer film-based waterproofing membrane. By setting an anti-adhesive layer, an adhesive layer and a polymer membrane base layer in the waterproof membrane, it combines sodium polyacrylate, manganese dioxide, magnesium silicate and polyacetic acid. Components such as vinyl ester enhance the bonding effect and physical barrier capability of the adhesive layer, forming a stronger puncture-resistant structure.
The puncture resistance and root puncture resistance of the waterproof membrane are significantly improved, extending the service life of the building and avoiding safety and quality accidents.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a root penetration resistant double overlapped double polymer membrane based waterproof coiled material and a preparation method thereof. Background Art
[0002] Waterproof membrane is a kind of building material product used in building walls, roofs and other places to prevent external rainwater or groundwater from leaking. It is the first barrier of waterproofing for the entire construction project and plays a vital role in the entire construction project. With the continuous expansion of urban construction, building gardens and planting green plants such as flowers on the roof surface has become the main means of purifying the air and improving and beautifying the environment.
[0003] Since plant roots grow rapidly, they can easily penetrate waterproofing membranes, which can cause roof leakage and even affect the structure of the building, leading to safety and quality accidents. Existing waterproofing membrane products cannot form a root system as a whole due to their single formula and structure, and do not have the ability to resist plant root penetration. Therefore, the development of a waterproofing membrane that is resistant to root penetration has very important practical significance and commercial value. Summary of the invention
[0004] The invention provides a root-penetration-resistant double-lapped double-polymer membrane-based waterproofing coiled material and a preparation method thereof, which solves the problem that the root-penetration-resistant performance of the waterproofing coiled material in the related art is poor.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention provides a root-penetration-resistant double-lapped double-polymer membrane-based waterproofing coiled material, comprising an anti-adhesive layer, a first adhesive layer, a first polymer membrane base layer, a second adhesive layer, a second polymer membrane base layer, a third adhesive layer and a separator film which are sequentially arranged from top to bottom, wherein the first polymer membrane base layer and the second polymer membrane base layer each independently comprise the following components in parts by weight: 60 to 80 parts of polyethylene terephthalate, 40 to 60 parts of polypropylene, 15 to 30 parts of magnesium silicate and 1 to 3 parts of an antioxidant;
[0007] The first adhesive layer, the second adhesive layer and the third adhesive layer each independently comprise the following components in parts by weight: 40-60 parts of asphalt, 30-40 parts of ethylene-vinyl acetate copolymer, 20-30 parts of styrene-butadiene-styrene copolymer, 5-10 parts of tackifier, and 1-3 parts of root inhibitor;
[0008] The viscosity increasing agent includes sodium polyacrylate and manganese dioxide.
[0009] As a further technical solution, the mass ratio of the sodium polyacrylate to manganese dioxide is 1:4 to 4:1.
[0010] When the mass ratio of sodium polyacrylate and manganese dioxide is 1:4~4:1, the puncture resistance and root penetration resistance of the waterproof membrane can be further enhanced.
[0011] As a further technical solution, the mass ratio of the sodium polyacrylate to manganese dioxide is 2:3.
[0012] When the mass ratio of sodium polyacrylate to manganese dioxide is 2:3, the waterproof membrane has better puncture resistance and root penetration resistance.
[0013] As a further technical solution, the magnesium silicate is polyvinyl acetate modified magnesium silicate.
[0014] By modifying magnesium silicate with polyvinyl acetate, it helps to increase the dispersion effect of magnesium silicate in the polymer membrane base layer, thereby further enhancing the puncture resistance and root penetration resistance of the waterproof membrane.
[0015] As a further technical solution, in the polyvinyl acetate modified magnesium silicate, the mass ratio of polyvinyl acetate to magnesium silicate is 2:13~4:11.
[0016] In polyvinyl acetate modified magnesium silicate, when the mass ratio of polyvinyl acetate to magnesium silicate is 2:13~4:11, the puncture resistance and root penetration resistance of the waterproof membrane can be further enhanced.
[0017] As a further technical solution, the preparation method of the polyvinyl acetate modified magnesium silicate is: dissolving polyvinyl acetate in acetone, adding magnesium silicate, mixing evenly, and drying to obtain the polyvinyl acetate modified magnesium silicate.
[0018] As a further technical solution, the antioxidant is one or more of antioxidant 4010, antioxidant DPPD, and antioxidant IPPD.
[0019] As a further technical solution, the root inhibitor is B2 root inhibitor or B5 root inhibitor.
[0020] As a further technical solution, the isolation film is one of a polyvinyl chloride film, a polyethylene film, and a polypropylene film.
[0021] As a further technical solution, the anti-sticking layer is a polyethylene film or a polypropylene film.
[0022] The present invention also provides a method for preparing the root penetration resistant double overlapped double polymer membrane-based waterproofing coiled material, comprising the following steps:
[0023] S1, firstly blending and extruding the components of the first polymer film base layer to obtain a first polymer film base layer sheet, and secondly blending and extruding the components of the second polymer film base layer to obtain a second polymer film base layer sheet;
[0024] S2, after softening the asphalt, adding ethylene-vinyl acetate copolymer, styrene-butadiene-styrene copolymer, tackifier and root inhibitor and mixing evenly to obtain an adhesive;
[0025] S3. Spray the adhesive on the surfaces of the first polymer film base sheet and the second polymer film base sheet in the upper and lower order of the first adhesive layer, the first polymer film base layer, the second adhesive layer, the second polymer film base layer and the third adhesive layer. Cover the upper surface of the first adhesive layer with a release layer and the lower surface of the third adhesive layer with an isolation film to obtain a double-lapped double polymer film-based waterproof membrane.
[0026] As a further technical solution, in step S1, during the first co-extrusion and the second co-extrusion, the extrusion temperatures are independently: 170-180°C in zone 1, 190-200°C in zone 2, and 210-220°C in zone 3.
[0027] As a further technical solution, in step S2, when the asphalt is softened, the temperature is 180-190°C.
[0028] The working principle and beneficial effects of the present invention are:
[0029] 1. In the present invention, the adhesive layer tackifier includes sodium polyacrylate and manganese dioxide, which increases the bonding effect of the adhesive layer through organic and inorganic synergistic enhancement, thereby improving the puncture resistance and root penetration resistance of the waterproof membrane. In addition, the addition of magnesium silicate in the polymer film base can improve the mechanical properties of the waterproof membrane and enhance the physical barrier effect, thereby enhancing the puncture resistance and root penetration resistance of the waterproof membrane. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] In the following embodiments and comparative examples, unless otherwise specified, the model of polyethylene terephthalate is RE5329, the model of styrene-butadiene-styrene copolymer is JH-7546, the model of polypropylene is HX-3700, the particle size of magnesium silicate is 45 μm, the model of polyvinyl acetate is LA-5T, the model of asphalt is 90# asphalt, the model of ethylene-vinyl acetate copolymer is BJ-806H, the molecular weight of sodium polyacrylate is 5000, the particle size of manganese dioxide is 13 μm, the thickness of the polyethylene film is 0.15 mm, and the thickness of the polypropylene film is 0.15 mm.
[0032] Example 1
[0033] The preparation method of the root-penetration-resistant double-lap double-polymer membrane-based waterproofing coiled material comprises the following steps:
[0034] S1. By weight, 60 parts of polyethylene terephthalate, 40 parts of polypropylene, 15 parts of magnesium silicate, and 1 part of antioxidant 4010 are blended and extruded to obtain a first polymer film base sheet, and 60 parts of polyethylene terephthalate, 40 parts of polypropylene, 15 parts of magnesium silicate, and 1 part of antioxidant 4010 are blended and extruded to obtain a second polymer film base sheet;
[0035] Wherein, during the first co-mixing extrusion, the temperature of the first zone is 170°C, the temperature of the second zone is 190°C, and the temperature of the third zone is 210°C; during the second co-mixing extrusion, the temperature of the first zone is 170°C, the temperature of the second zone is 190°C, and the temperature of the third zone is 210°C;
[0036] S2, after softening 40 parts of asphalt at 180° C., add 30 parts of ethylene-vinyl acetate copolymer, 20 parts of styrene-butadiene-styrene copolymer, 0.5 parts of sodium polyacrylate, 4.5 parts of manganese dioxide, and 1 part of B2 root inhibitor and mix well to obtain an adhesive;
[0037] S3. Spray the adhesive on the surfaces of the first polymer film base sheet and the second polymer film base sheet in the upper and lower order of the first adhesive layer, the first polymer film base layer, the second adhesive layer, the second polymer film base layer and the third adhesive layer. Cover the upper surface of the first adhesive layer with a polyethylene film and the lower surface of the third adhesive layer with a polypropylene film to obtain a double-lapped double polymer film-based waterproof membrane.
[0038] Example 2
[0039] The preparation method of the root-penetration-resistant double-lap double-polymer membrane-based waterproofing coiled material comprises the following steps:
[0040] S1. By weight, 80 parts of polyethylene terephthalate, 60 parts of polypropylene, 30 parts of magnesium silicate, and 3 parts of antioxidant 4010 are blended and extruded to obtain a first polymer film base sheet, and 80 parts of polyethylene terephthalate, 60 parts of polypropylene, 30 parts of magnesium silicate, and 3 parts of antioxidant 4010 are blended and extruded to obtain a second polymer film base sheet;
[0041] Wherein, during the first co-mixing extrusion, the temperature of the first zone is 180°C, the temperature of the second zone is 200°C, and the temperature of the third zone is 220°C; during the second co-mixing extrusion, the temperature of the first zone is 180°C, the temperature of the second zone is 200°C, and the temperature of the third zone is 220°C;
[0042] S2, after softening 60 parts of asphalt at 190° C., add 40 parts of ethylene-vinyl acetate copolymer, 30 parts of styrene-butadiene-styrene copolymer, 1 part of sodium polyacrylate, 9 parts of manganese dioxide, and 3 parts of B2 root inhibitor and mix well to obtain an adhesive;
[0043] S3. Spray the adhesive on the surfaces of the first polymer film base sheet and the second polymer film base sheet in the upper and lower order of the first adhesive layer, the first polymer film base layer, the second adhesive layer, the second polymer film base layer and the third adhesive layer. Cover the upper surface of the first adhesive layer with a polyethylene film and the lower surface of the third adhesive layer with a polypropylene film to obtain a double-lapped double polymer film-based waterproof membrane.
[0044] Example 3
[0045] The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight portion of sodium polyacrylate is 9 parts, and the weight portion of manganese dioxide is 1 part.
[0046] Example 4
[0047] The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight portion of sodium polyacrylate is 2 parts, and the weight portion of manganese dioxide is 8 parts.
[0048] Example 5
[0049] The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight portion of sodium polyacrylate is 8 parts, and the weight portion of manganese dioxide is 2 parts.
[0050] Example 6
[0051] The only difference between this embodiment and embodiment 2 is that, in this embodiment, the weight parts of sodium polyacrylate are 4 parts, and the weight parts of manganese dioxide are 6 parts.
[0052] Example 7
[0053] The only difference between this embodiment and embodiment 6 is that in this embodiment, the magnesium silicate is polyvinyl acetate modified magnesium silicate, and the preparation method of polyvinyl acetate modified magnesium silicate is: dissolving 3 parts of polyvinyl acetate in 20 parts of acetone, adding 27 parts of magnesium silicate, mixing evenly, and drying to obtain polyvinyl acetate modified magnesium silicate.
[0054] Example 8
[0055] The only difference between this embodiment and embodiment 7 is that, in this embodiment, the weight parts of polyvinyl acetate are 9 parts and the weight parts of magnesium silicate are 21 parts.
[0056] Example 9
[0057] The only difference between this embodiment and embodiment 7 is that, in this embodiment, the weight parts of polyvinyl acetate are 4 parts and the weight parts of magnesium silicate are 26 parts.
[0058] Example 10
[0059] The only difference between this embodiment and embodiment 7 is that, in this embodiment, the weight parts of polyvinyl acetate are 8 parts and the weight parts of magnesium silicate are 22 parts.
[0060] Comparative Example 1
[0061] The only difference between this comparative example and Example 1 is that in this comparative example, magnesium silicate is not added.
[0062] Comparative Example 2
[0063] The difference between this comparative example and Example 1 is that in this comparative example, sodium polyacrylate is not added and the weight portion of manganese dioxide added is 5 parts.
[0064] Comparative Example 3
[0065] The difference between this comparative example and Example 1 is that in this comparative example, manganese dioxide is not added and the weight portion of sodium polyacrylate added is 5 parts.
[0066] Comparative Example 4
[0067] The only difference between this comparative example and Example 1 is that in this comparative example, manganese dioxide and sodium polyacrylate are not added.
[0068] Experimental Example 1: Puncture resistance
[0069] The double-lapped double polymer membrane-based waterproof membranes prepared in Examples 1 to 10 and Comparative Examples 1 to 4 were tested for puncture resistance according to GB / T23457-2017 "Pre-laid Waterproof Membrane". The test results are shown in Table 1 below.
[0070] Table 1 Puncture resistance test results
[0071]
[0072] The comparison between Example 1 and Comparative Example 1 shows that the addition of magnesium silicate in the polymer film base layer can improve the puncture resistance of the waterproof coiled material. The comparison between Example 1 and Comparative Examples 2-4 shows that the puncture resistance of the waterproof coiled material is improved by the synergistic effect of sodium polyacrylate and manganese dioxide. The comparison between Examples 2-3 and Examples 4-6 shows that when the mass ratio of sodium polyacrylate and manganese dioxide is 1:4-4:1, the puncture resistance of the waterproof coiled material can be further improved. The comparison between Example 6 and Examples 4-5 shows that when the mass ratio of sodium polyacrylate and manganese dioxide is 2:3, the waterproof coiled material has a more excellent puncture resistance. The comparison between Example 6 and Examples 7-10 shows that by modifying magnesium silicate with polyvinyl acetate, it is helpful to further improve the puncture resistance of the waterproof coiled material. The comparison between Examples 9-10 and Examples 7-8 shows that when the mass ratio of polyvinyl acetate and magnesium silicate is 2:13-4:11, the puncture resistance of the waterproof coiled material can be further improved.
[0073] Experimental Example 2 Root penetration resistance
[0074] The double-lapped double polymer membrane-based waterproof membrane prepared in Examples 1 to 10 was tested for root penetration resistance according to GB / T 35468-2017 "Root penetration resistant waterproof membrane for planted roofs". The test period was 6 months, and the test results are shown in Table 2 below.
[0075] Table 2 Root penetration resistance test results
[0076]
[0077] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A root-penetration-resistant double-lapped double polymer membrane-based waterproofing coiled material, comprising an anti-adhesive layer, a first adhesive layer, a first polymer membrane base layer, a second adhesive layer, a second polymer membrane base layer, a third adhesive layer and an isolation membrane arranged in sequence from top to bottom, characterized in that: The first polymer film base layer and the second polymer film base layer each independently comprise the following components in parts by weight: 60-80 parts of polyethylene terephthalate, 40-60 parts of polypropylene, 15-30 parts of magnesium silicate, and 1-3 parts of an antioxidant; The first adhesive layer, the second adhesive layer and the third adhesive layer each independently comprise the following components in parts by weight: 40-60 parts of asphalt, 30-40 parts of ethylene-vinyl acetate copolymer, 20-30 parts of styrene-butadiene-styrene copolymer, 5-10 parts of tackifier, and 1-3 parts of root inhibitor; The viscosity increasing agent includes sodium polyacrylate and manganese dioxide; The magnesium silicate is polyvinyl acetate modified magnesium silicate.
2. The root penetration resistant double overlapped double polymer membrane based waterproofing coiled material according to claim 1, characterized in that: The mass ratio of the sodium polyacrylate to manganese dioxide is 1:4 to 4:
1.
3. The root penetration resistant double overlapped double polymer membrane based waterproofing coiled material according to claim 2, characterized in that: The mass ratio of the sodium polyacrylate to manganese dioxide is 2:
3.
4. The root penetration resistant double overlap double polymer membrane based waterproofing coiled material according to claim 1, characterized in that: In the polyvinyl acetate modified magnesium silicate, the mass ratio of polyvinyl acetate to magnesium silicate is 2:13-4:
11.
5. The root penetration resistant double overlap double polymer membrane based waterproofing coiled material according to claim 1, characterized in that: The preparation method of the polyvinyl acetate modified magnesium silicate is as follows: dissolving polyvinyl acetate in acetone, adding magnesium silicate, mixing evenly, and drying to obtain the polyvinyl acetate modified magnesium silicate.
6. The root penetration resistant double overlapped double polymer membrane based waterproofing coiled material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 4010, antioxidant DPPD, and antioxidant IPPD.
7. The root penetration resistant double overlapped double polymer membrane based waterproofing coiled material according to claim 1, characterized in that: The root inhibitor is B2 root inhibitor or B5 root inhibitor.
8. A method for preparing the root penetration resistant double overlapped double polymer membrane-based waterproofing coiled material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, firstly blending and extruding the components of the first polymer film base layer to obtain a first polymer film base layer sheet, and secondly blending and extruding the components of the second polymer film base layer to obtain a second polymer film base layer sheet; S2, after softening the asphalt, adding ethylene-vinyl acetate copolymer, styrene-butadiene-styrene copolymer, tackifier and root inhibitor and mixing evenly to obtain an adhesive; S3. Spray the adhesive on the surfaces of the first polymer film base sheet and the second polymer film base sheet in the upper and lower order of the first adhesive layer, the first polymer film base layer, the second adhesive layer, the second polymer film base layer and the third adhesive layer. Cover the upper surface of the first adhesive layer with a release layer and the lower surface of the third adhesive layer with an isolation film to obtain a double-lapped double polymer film-based waterproof membrane.
9. The method for preparing a root-penetration-resistant double-lap double-polymer membrane-based waterproofing coiled material according to claim 8, characterized in that: In step S1, during the first co-extrusion and the second co-extrusion, the extrusion temperatures are independently: 170-180°C in the first zone, 190-200°C in the second zone, and 210-220°C in the third zone.