A magnesium alloy sheet with high plasticity and high work hardening and its preparation method

By adding Zn, Li, and Gd to magnesium alloys, magnesium alloy thin sheets with multi-directional bias textures were prepared, which solved the problem of poor deformation ability of magnesium alloy sheets at room temperature, achieved high plasticity and high work hardening ability, and improved the performance of magnesium alloy thin sheets.

CN118028677BActive Publication Date: 2026-11-17YUNNAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410130446.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-31
Publication Date
2026-11-17
Estimated Expiration
2044-01-31

AI Technical Summary

Technical Problem

Magnesium alloy sheets have poor deformation capacity at room temperature and are prone to forming a strong base surface texture of c-axis∥ND during secondary processing, which limits their deep processing and forming capabilities, increases production costs, and fails to meet the plasticity requirements of complex products.

Method used

By adding 1-2% Zn, 0.3-1.2% Li and 0.2-1% Gd to magnesium alloy, a magnesium alloy sheet with multi-directional bias texture was prepared. Vacuum melting, homogenization annealing and hot extrusion processes were used to form fine grains and multi-directional bias texture, which activated more non-basal plane slip.

Benefits of technology

It achieves high plasticity and high work hardening ability of magnesium alloy thin plates at room temperature, with yield strength exceeding 108MPa, tensile strength exceeding 290MPa, and room temperature elongation exceeding 36%, which is significantly better than commercial magnesium alloy AZ31.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118028677B_ABST
    Figure CN118028677B_ABST
Patent Text Reader

Abstract

This invention discloses a high-plasticity, high-work-hardening magnesium alloy sheet and its preparation method, comprising Zn 1-2%; Li 0.3-1.2%; Gd 0.2-1%; with the balance being Mg. The magnesium alloy sheet prepared by this invention has fine grains, with an average grain size of 8-10 μm. Its yield strength exceeds 108 MPa, tensile strength exceeds 290 MPa, and room temperature elongation exceeds 36%. The work-hardening capacity (tensile strength - yield strength) and room temperature elongation of this alloy sheet are significantly superior to the most widely used commercial magnesium alloy AZ31.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of magnesium alloy technology, and in particular to a magnesium alloy sheet with high plasticity and high work hardening and its preparation method. Background Technology

[0002] As a major magnesium resource country, my country boasts 22.5% of the world's magnesium reserves, ranking first globally. Magnesium alloys possess numerous advantages, including low density, high specific strength, excellent damping performance, environmental friendliness, and 100% recyclability. They have broad application prospects in numerous fields such as the automotive industry, aerospace, rail transportation, military industry, and electronic communications, and are hailed as one of the most promising green structural materials of the 21st century. However, magnesium alloys have a close-packed hexagonal structure, resulting in poor deformability at room temperature. Furthermore, magnesium alloy sheets formed in a single process are prone to developing a c-axis∥ND type strong basal plane texture during secondary processing, limiting their deep processing capabilities. Many magnesium alloy sheets require further heating for deformation, significantly increasing the production cost of magnesium products. Currently, the most widely used commercial magnesium alloy, AZ31, has few activated slip systems at room temperature, only basal plane slip can be activated, and its elongation is low, failing to meet the plasticity requirements of complex magnesium alloy products in production and daily life. Therefore, developing a new type of magnesium alloy sheet with high plasticity and high work hardening at room temperature is of great significance for expanding the application range of magnesium alloy products. Summary of the Invention

[0003] To overcome the above deficiencies, the present invention provides a magnesium alloy sheet with high plasticity and high work hardening at room temperature to solve the problems in the background art.

[0004] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows:

[0005] A high-plasticity, high-work-hardening magnesium alloy sheet, by mass percentage:

[0006] Zn 1-2%;

[0007] Li 0.3–1.2%;

[0008] Gd 0.2-1%;

[0009] The balance is Mg.

[0010] As a preferred technical solution, the high-plasticity, high-work-hardening magnesium alloy sheet, by mass percentage:

[0011] Zn 1.8%;

[0012] Li 0.9%;

[0013] Gd 0.8%;

[0014] The balance is Mg.

[0015] As a preferred technical solution, the Zn is a Zn ingot.

[0016] As a preferred technical solution, the Gd is a Gd ingot.

[0017] As a preferred technical solution, the Mg is Mg ingot.

[0018] As a preferred technical solution, the Li is a Mg-3Li master alloy.

[0019] As a preferred technical solution, the average grain size of the magnesium alloy sheet is 8-10 μm.

[0020] The present invention also provides a method for preparing the aforementioned high-plasticity, high-work-hardening magnesium alloy sheet, comprising the steps of:

[0021] 1) Ingredients

[0022] The surface oxide scale and impurities of the elemental metals Mg ingot, Zn ingot, Gd ingot, and Mg-3Li master alloy are removed by grinding and polishing. Then, according to the mass percentage = Zn: 1-2%, Li: 0.3-1.2%, Gd: 0.2-1%, and the remainder is Mg, the raw materials are weighed.

[0023] 2) Smelting

[0024] The weighed mixture from the above steps is placed in a vacuum melting furnace. The pressure inside the furnace is reduced to 200 Pa using a mechanical pump, and the temperature inside the furnace is gradually increased to 390-415°C. The furnace is heated for 10-25 minutes, and then 99% carbon dioxide and 1% sulfur hexafluoride are introduced into the furnace. The temperature of the vacuum melting furnace is further increased to 730-760°C to melt the various raw materials. After holding the temperature for 50 minutes, the temperature of the vacuum melting furnace is reduced for casting. The resulting magnesium alloy ingot is machined to φ=85mm using a lathe.

[0025] 3) Homogenization annealing treatment

[0026] The obtained ingot with a diameter of 85 mm was placed in an annealing furnace and held at 320-490℃ for 6-12 hours to remelt the second phase, thereby eliminating element segregation during the casting process and improving the uniformity of the microstructure.

[0027] 4) Hot extrusion

[0028] The alloy ingot processed in step 3 is preheated at 420-450°C for half an hour, and then hot-extruded in a 1600-ton horizontal extrusion press at a temperature of 420-460°C to extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2 mm, thus obtaining a magnesium alloy sheet with high plasticity and high work hardening at room temperature.

[0029] As a preferred technical solution, in step 1), the raw materials are weighed according to the mass percentages of Zn 1.8%, Li 0.9%, Gd 0.8%, and the balance being Mg.

[0030] As a preferred technical solution, the average grain size of the magnesium alloy sheet is 8-10 μm.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] (1) By adding fewer alloying elements to magnesium, production costs can be effectively reduced, and the resulting alloy sheet exhibits excellent performance. Firstly, the fine grains in the sheet contribute to improved strength and plasticity. Secondly, the sheet exhibits low texture strength and forms a “c-axis / / TD split texture + ND axially symmetric ring texture,” as shown in the image. Figure 1 As shown. This is because Li and Gd not only weaken the texture but also allow the texture to be biased along different directions. Adding Li to magnesium alloys can form a biased texture along the TD direction, while adding Gd and rolling can form a biased texture along the ED direction. Therefore, adding Li and Gd simultaneously in equal proportions to magnesium alloys will form a special multi-directional biased texture. This texture gives the sheet metal better coordination during plastic deformation at room temperature.

[0033] (2) Zn, Li, and Gd can all reduce the axial ratio of magnesium, enabling the sheet to activate more non-basal slip at room temperature, enriching the plastic deformation mechanism and improving room temperature plasticity. Furthermore, the more balanced the activation ratio of basal and non-basal slip, the higher the work hardening rate. In addition, the interaction of multiple elements makes it easier to control the stacking fault energy of the alloy, resulting in more stacking faults during plastic deformation. Dislocations accumulate at stacking fault sites, greatly enhancing the room temperature work hardening capability. Therefore, under the combined influence of multiple conditions, the magnesium alloy sheet obtained in this patent possesses excellent room temperature plasticity and high work hardening capability, with a room temperature elongation exceeding 36%. Figure 2 As shown.

[0034] Due to the adoption of the above technical solution, a high-plasticity, high-work-hardening magnesium alloy sheet and its preparation method are obtained. The composition is: Zn 1-2%; Li 0.3-1.2%; Gd 0.2-1%; balance Mg. The magnesium alloy sheet prepared by this invention has fine grains, with an average grain size of 8-10 μm. Its yield strength exceeds 108 MPa, tensile strength exceeds 290 MPa, and room temperature elongation exceeds 36%. The work-hardening capacity (tensile strength - yield strength) and room temperature elongation of this alloy sheet are significantly superior to the most widely used commercial magnesium alloy AZ31. Attached Figure Description

[0035] Figure 1 EBSD analysis of alloy plates;

[0036] Figure 2 Room temperature tensile curve of alloy sheet. Detailed Implementation

[0037] A high-plasticity, high-work-hardening magnesium alloy sheet, by mass percentage:

[0038] Zn 1-2%;

[0039] Li 0.3–1.2%;

[0040] Gd 0.2-1%;

[0041] The balance is Mg.

[0042] The aforementioned high-plasticity, high-work-hardening magnesium alloy sheet, by mass percentage:

[0043] Zn 1.8%;

[0044] Li 0.9%;

[0045] Gd 0.8%;

[0046] The balance is Mg.

[0047] The Zn is a Zn ingot.

[0048] The Gd is a Gd ingot.

[0049] The Mg is Mg ingot.

[0050] The Li is a Mg-3Li master alloy.

[0051] The average grain size of the magnesium alloy sheet is 8–10 μm.

[0052] The present invention also provides a method for preparing the aforementioned high-plasticity, high-work-hardening magnesium alloy sheet, comprising the steps of:

[0053] 1) Ingredients

[0054] The surface oxide scale and impurities of the elemental metals Mg ingot, Zn ingot, Gd ingot, and Mg-3Li master alloy are removed by grinding and polishing. Then, according to the mass percentage = Zn: 1-2%, Li: 0.3-1.2%, Gd: 0.2-1%, and the remainder is Mg, the raw materials are weighed.

[0055] 2) Smelting

[0056] The weighed mixture from the above steps is placed in a vacuum melting furnace. The pressure inside the furnace is reduced to 200 Pa using a mechanical pump, and the temperature inside the furnace is gradually increased to 390-415°C. The furnace is heated for 10-25 minutes, and then 99% carbon dioxide and 1% sulfur hexafluoride are introduced into the furnace. The temperature of the vacuum melting furnace is further increased to 730-760°C to melt the various raw materials. After holding the temperature for 50 minutes, the temperature of the vacuum melting furnace is reduced for casting. The resulting magnesium alloy ingot is machined to φ=85mm using a lathe.

[0057] 3) Homogenization annealing treatment

[0058] The obtained ingot with a diameter of 85 mm was placed in an annealing furnace and held at 320-490℃ for 6-12 hours to remelt the second phase, thereby eliminating element segregation during the casting process and improving the uniformity of the microstructure.

[0059] 4) Hot extrusion

[0060] The alloy ingot processed in step 3 is preheated at 420-450°C for half an hour, and then hot-extruded in a 1600-ton horizontal extrusion press at a temperature of 420-460°C to extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2 mm, thus obtaining a magnesium alloy sheet with high plasticity and high work hardening at room temperature.

[0061] In step 1), the raw materials are weighed according to the mass percentages of Zn 1.8%, Li 0.9%, Gd 0.8%, with the balance being Mg.

[0062] The average grain size of the magnesium alloy sheet is 8–10 μm.

[0063] The present invention will be further illustrated below with reference to embodiments. In the following detailed description, only certain exemplary embodiments of the invention are described by way of illustration. Undoubtedly, those skilled in the art will recognize that various modifications can be made to the described embodiments without departing from the spirit and scope of the invention. Therefore, the drawings and description are illustrative in nature and not intended to limit the scope of the claims.

[0064] Example 1

[0065] 900g of Mg blocks, 470g of Mg-3Li master alloy, 28g of Zn blocks, and 14g of Gd blocks were placed in a vacuum induction melting furnace. The furnace temperature was gradually raised to 410±10℃ and heated for 15 minutes. Then, 99% carbon dioxide and 1% sulfur hexafluoride by volume were introduced into the furnace, and the temperature of the vacuum melting furnace was further increased to 745±10℃ to melt the various raw materials. After holding at this temperature for 50 minutes, the temperature of the vacuum melting furnace was lowered for casting. The resulting magnesium alloy ingot was machined to φ=85mm using a lathe.

[0066] The obtained magnesium alloy ingot was homogenized at 395±10℃ for 12 hours, and then preheated at 435±10℃ for half an hour. It was then hot-extruded in a 1600-ton horizontal extrusion press to finally extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2mm.

[0067] Microstructural analysis of the 2mm extruded sheet from the above steps revealed uniform grain size and a split texture distributed transversely. Room temperature tensile testing showed a yield strength exceeding 108.1 MPa, a tensile strength exceeding 292.5 MPa, a room temperature elongation of 36.3%, and a yield-to-tensile ratio of 0.37.

[0068] Example 2

[0069] 1000g of Mg block, 450g of Mg-3Li master alloy, 20g of Zn block, and 12g of Gd block were placed in a vacuum induction melting furnace. The furnace temperature was gradually raised to 400±10℃ and heated for 15 minutes. Then, 99% carbon dioxide and 1% sulfur hexafluoride were introduced into the furnace, and the temperature of the vacuum melting furnace was further increased to 740±10℃ to melt the various raw materials. After holding at this temperature for 50 minutes, the temperature of the vacuum melting furnace was lowered for casting. The resulting magnesium alloy ingot was machined to φ=85mm using a lathe.

[0070] The obtained magnesium alloy ingot was homogenized at 390±10℃ for 12 hours, and then the alloy ingot was preheated at 430±10℃ for half an hour. It was then hot-extruded in a 1600-ton horizontal extrusion press, and finally the original alloy ingot was extruded into a magnesium alloy sheet with a thickness of 2mm.

[0071] Microstructural analysis of the 2mm sheet after extrusion in the above steps revealed uniform grain size and a split texture distributed transversely. Room temperature tensile testing showed a yield strength of 111.7 MPa, a tensile strength exceeding 291.4 MPa, a room temperature elongation of 36.8%, and a yield-to-tensile ratio of 0.38.

[0072] Example 3

[0073] 900g of Mg blocks, 500g of Mg-3Li master alloy, 30g of Zn blocks, and 15g of Gd blocks were placed in a vacuum induction melting furnace. The furnace temperature was gradually raised to 405±10℃ and heated for 15 minutes. Then, 99% carbon dioxide and 1% sulfur hexafluoride were introduced into the furnace, and the temperature of the vacuum melting furnace was further increased to 750±10℃ to melt the various raw materials. After holding at this temperature for 50 minutes, the temperature of the vacuum melting furnace was lowered for casting. The resulting magnesium alloy ingot was machined to φ=85mm using a lathe.

[0074] The obtained magnesium alloy ingot was homogenized at 390±10℃ for 12 hours, then preheated at 430±10℃ for half an hour, and then hot extruded under a 1600-ton horizontal extrusion press to finally extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2mm.

[0075] Microstructural analysis of the 2mm sheet material after extrusion in the above steps revealed fine grains and a split texture distributed transversely. Room temperature tensile testing showed a yield strength of 108.6 MPa, a tensile strength of 298.6 MPa, a room temperature elongation exceeding 36.2%, and a yield-to-tensile ratio of 0.36.

[0076] Example 4

[0077] 950g of Mg block, 450g of Mg-3Li master alloy, 30g of Zn block, and 10g of Gd block were placed in a vacuum induction melting furnace. The furnace temperature was gradually raised to 400±10℃ and heated for 10 minutes. Then, 99% carbon dioxide and 1% sulfur hexafluoride were introduced into the furnace, and the temperature of the vacuum melting furnace was further increased to 740±10℃ to melt the various raw materials. After holding at this temperature for 50 minutes, the temperature of the vacuum melting furnace was lowered for casting. The resulting magnesium alloy ingot was machined to φ=85mm using a lathe.

[0078] The obtained magnesium alloy ingot was homogenized at 330±10℃ for 8 hours, then the alloy ingot was preheated at 430±10℃ for half an hour, and then hot extruded under a 1600-ton horizontal extrusion press to finally extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2mm.

[0079] Microstructural analysis of the 2mm sheet material after extrusion in the above steps revealed fine grains and a split texture distributed laterally. Room temperature tensile testing showed a yield strength of 112.2 MPa, a tensile strength of 293.6 MPa, a room temperature elongation exceeding 36.4%, and a yield-to-tensile ratio of 0.38.

[0080] Example 5

[0081] 900g of Mg blocks, 420g of Mg-3Li master alloy, 25g of Zn blocks, and 14g of Gd blocks were placed in a vacuum induction melting furnace. The furnace temperature was gradually raised to 405±10℃ and heated for 25 minutes. Then, 99% carbon dioxide and 1% sulfur hexafluoride were introduced into the furnace, and the temperature of the vacuum melting furnace was further increased to 750±10℃ to melt the various raw materials. After holding at this temperature for 50 minutes, the temperature of the vacuum melting furnace was lowered for casting. The resulting magnesium alloy ingot was machined to φ=85mm using a lathe.

[0082] The obtained magnesium alloy ingot was homogenized at 480±10℃ for 6 hours, then preheated at 440±10℃ for half an hour, and then hot extruded under a 1600-ton horizontal extrusion press to finally extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2mm.

[0083] Microstructural analysis of the 2mm sheet material after extrusion in the above steps revealed fine grains and a split texture distributed laterally. Room temperature tensile testing showed a yield strength of 115.8 MPa, a tensile strength of 298.6 MPa, a room temperature elongation exceeding 36.1%, and a yield-to-tensile ratio of 0.39.

[0084] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.

Claims

1. A magnesium alloy sheet with high plasticity and high work hardening, characterized in that, By mass percentage: Zn 1.8%; Li 0.9%; Gd 0.8%; The balance is Mg; A method for preparing magnesium alloy thin sheets with high plasticity and high work hardening includes the following steps: 1) Ingredients The surface oxide scale and impurities of the elemental metals Mg ingot, Zn ingot, Gd ingot, and Mg-3Li master alloy were removed by grinding and polishing machine. Then, according to the mass percentage = Zn: 1.8%, Li: 0.9%, Gd: 0.8%, and the remainder is Mg, the raw materials were weighed. 2) Smelting The weighed mixture from the above steps is placed in a vacuum melting furnace. The pressure inside the furnace is reduced to 200 Pa using a mechanical pump, and the temperature inside the furnace is gradually increased to 390-415℃. The furnace is heated for 10-25 minutes, and then 99% carbon dioxide and 1% sulfur hexafluoride are introduced into the furnace. The temperature of the vacuum melting furnace is further increased to 730-760℃ to melt the various raw materials. After holding the temperature for 50 minutes, the temperature of the vacuum melting furnace is reduced for casting. The resulting magnesium alloy ingot is machined to φ=85mm using a lathe. 3) Homogenization annealing treatment The obtained ingot with a diameter of 85 mm was placed in an annealing furnace and held at 320-490℃ for 6-12 hours to remelt the second phase, thereby eliminating element segregation during the casting process and improving the uniformity of the microstructure. 4) Hot extrusion The alloy ingot processed in step 3 is preheated at 420-450°C for half an hour, and then hot-extruded in a 1600-ton horizontal extrusion press at a temperature of 420-460°C to extrude the original alloy ingot into a magnesium alloy sheet with a thickness of 2 mm, thus obtaining a magnesium alloy sheet with high plasticity and high work hardening at room temperature.

2. The high-plasticity, high-work-hardening magnesium alloy sheet as described in claim 1, characterized in that: The average grain size of the magnesium alloy sheet is 8–10 μm.

Citation Information

Patent Citations

  • Low-cost high-strength high-toughness high-thermal conductivity wrought magnesium alloy and preparation method thereof

    CN105755340A

  • High-plasticity and high-formability magnesium alloy plate with annular divergent texture and preparation method of high-plasticity and high-formability magnesium alloy plate

    CN113444945A