Modified wool fiber, preparation method, composite foaming material and preparation method thereof

By using enzyme treatment of wool fibers to form a porous structure and mix it with titanate coupling agent, and foaming with aqueous resin, it solves the problems of low strength and flammability of water-based polyurethane foaming materials, significantly improves porosity and performance, and achieves the Efficient utilization of waste wool resources.

CN118029165BActive Publication Date: 2024-12-06SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410437778.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-12-06
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

The existing water-based polyurethane foaming materials are limited in their application due to low strength, low porosity, and flammability. In particular, animal biomass wool fibers have been studied in this field, which has failed to effectively improve their porosity and mechanical properties. Thermal insulation and flame retardant properties.

Method used

Modified wool fibers were prepared by enzymatic treatment with cysteine ​​desulfurase to form a porous structure and mixed with a chelating titanate coupling agent, which was then blended with an aqueous resin and at room temperature. Fully foamed under the ground to form a composite foamed material.

Benefits of technology

The porosity, mechanical properties, flame retardant properties and thermal insulation properties of composite foam materials have been significantly improved, and the effective utilization of waste wool resources has been achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of foaming materials, and specifically relates to modified wool fibers, preparation methods, composite foaming materials and preparation methods thereof. In the present invention, after the wool fibers are opened, cysteine ​​desulfurase is used for processing, and the enzyme acts on the cortical layer of the wool fibers to decompose cysteine, so that gaps are formed on the surface of the wool fibers. The obtained modified wool fibers are porous wool fibers, which can improve the porosity of the composite foaming materials when applied to composite foaming materials, and the composite foaming materials finally obtained exhibit good mechanical properties, flame retardant properties, heat insulation properties and thermal insulation properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming materials, and in particular relates to modified wool fiber, a preparation method, a composite foaming material and a preparation method thereof. Background Art

[0002] Waterborne polyurethane foam is an important synthetic material with the characteristics of light weight, high elasticity, sound absorption, and breathability. It can be made into soft, hard, and semi-hard foam materials according to the different raw materials and formulas used. It is widely used in papermaking, construction, packaging, automotive industry, etc. Among them, the soft waterborne polyurethane foam with an open-cell structure is limited in application due to its low strength, low porosity, flammability, and other problems.

[0003] The performance of waterborne polyurethane foam materials can be improved by adding functional fillers. For example, nanoparticles and glass fibers are commonly used for reinforcement, and flame retardants such as magnesium-aluminum hydrotalcite, organic clay and melamine are commonly used to improve their flame retardant properties. In recent years, biomass has also been used for compounding with polyurethane foam materials due to its wide source, low cost and easy processing. However, research has mainly focused on plant biomass, such as cellulose, lignin and starch, and less research has been done on animal biomass (such as wool fibers). There has been no report on the use of waste wool fibers to enhance the porosity, mechanical properties, thermal insulation properties and flame retardant properties of waterborne resin foam materials.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The present invention aims to solve at least one of the above technical problems and proposes modified wool fiber, a preparation method, a composite foaming material and a preparation method thereof.

[0006] To achieve the above object, the first technical solution provided by the present invention is:

[0007] The preparation method of modified wool fiber comprises the following steps: opening pretreated wool fiber, performing enzyme treatment with cysteine ​​desulfurase, and washing with water to obtain enzyme-treated wool fiber;

[0008] The enzyme-treated wool fiber and the chelated titanate coupling agent solution are mixed and reacted, and the modified wool fiber is obtained by filtering and drying.

[0009] Preferably, the dosage of the cysteine ​​desulfurase is 0.1%-10% of the mass of the wool fiber.

[0010] Preferably, the enzyme treatment temperature is 20-55°C and the time is 0.5-2h.

[0011] Preferably, the amount of the chelated titanate coupling agent is 0.5%-5% of the mass of the wool fiber.

[0012] Preferably, the chelate titanate coupling agent comprises any one or more of ethyl tris(β-aminopropionic acid) titanium (EAT), ethyl amide triacetic acid titanate (EATT), di(dihydroxyphenyl) diisobutyrate titanium, and titanium n-butoxide.

[0013] Preferably, the mixing reaction is carried out at room temperature for 1-2 hours.

[0014] Preferably, the pretreated wool fiber is obtained by crushing the wool fiber into 20-200 meshes.

[0015] The present invention also provides modified wool fibers obtained by any of the above preparation methods.

[0016] The second technical solution provided by the present invention is:

[0017] A composite foam material, comprising the above modified wool fiber and water-based resin, wherein the mass ratio of the modified wool fiber to the water-based resin is 1:(1-10);

[0018] The water-based resin includes any one or more of water-based polyurethane, polyvinyl alcohol resin, polyacrylic acid resin, polyvinyl acid resin, styrene-butadiene resin and the like.

[0019] The third technical solution provided by the present invention is:

[0020] The preparation method of the composite foam material comprises the following steps: blending the modified wool fiber with the water-based resin, stirring the mixture at a rate of 1000-5000 r / min for 5-30 minutes at room temperature to fully foam the mixture, and drying the mixture.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The invention uses cysteine ​​desulfurase to treat wool fibers after fiber opening. The enzyme acts on the cortical layer of the wool fibers to decompose cysteine, so that voids are formed on the surface of the wool fibers. The obtained modified wool fibers are porous wool fibers. When the modified wool fibers are applied to composite foaming materials, the porosity of the composite foaming materials can be improved. The composite foaming materials finally obtained exhibit good mechanical properties, flame retardant properties, heat insulation properties and thermal insulation properties.

[0023] The wool fiber raw material of the present invention can be waste wool fiber, thus realizing a technology for the bulk resource utilization of waste wool. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments.It should be understood that these descriptions are exemplary only, and are not intended to limit the scope of the present invention.In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.Unspecified conditions in the embodiments are carried out according to the conditions of normal conditions or manufacturer recommendations.Reagents used or instruments that do not specify manufacturers are conventional products that can be purchased and obtained commercially.

[0025] The first embodiment of the present invention provides a method for preparing modified wool fibers, which comprises opening pretreated wool fibers, performing enzyme treatment with cysteine ​​desulfurase, and washing the pretreated wool fibers to obtain enzyme-treated wool fibers;

[0026] The enzyme-treated wool fiber and the chelated titanate coupling agent solution are mixed and reacted, and the modified wool fiber is obtained by filtering and drying.

[0027] The embodiment of the present invention can increase the surface roughness of wool by opening the wool fiber, which not only increases the surface area and active sites of the wool fiber to promote the penetration and action of the subsequent enzyme preparation, but also enables the wool fiber to be mechanically interlocked with the surface of the water-based resin when it is subsequently compounded with the water-based resin, thereby improving the mechanical properties of the foaming material. The opened wool fiber is treated with cysteine ​​desulfurase, which acts on the cortical layer of the wool fiber to decompose cysteine, so that a large number of pores are generated inside the wool fiber to obtain a porous wool fiber. When it is compounded with a foaming material, the porosity of the foaming material can be significantly improved, and the performance of the foaming material such as heat insulation, heat preservation, and flame retardancy can be improved. The wool fiber after enzyme treatment is mixed with a chelating titanate coupling agent solution to achieve chemical modification, which can further increase the surface active sites of the wool fiber and improve the interface compatibility between wool and resin.

[0028] In some preferred embodiments, the pretreatment is to crush the wool fibers into 20-200 meshes.

[0029] The invention pulverizes wool fibers to homogenize the wool fibers. Controlling the particle size after pulverization within this range can control the fiber aspect ratio and enhance the mechanical properties of the water-based resin.

[0030] In some preferred embodiments, the amount of cysteine ​​desulfurase is 0.1%-10% of the mass of the wool fiber, the temperature of the enzyme treatment is 20-55°C, and the time is 0.5h-2h. Experimental verification shows that when the amount of cysteine ​​desulfurase in the present invention is 1%-5% of the mass of the wool fiber, the porosity of the modified wool fiber used in the composite foaming material is the highest.

[0031] The mixed reaction is a common method for modification reaction of titanate coupling agents and does not need to be specifically limited. The reaction temperature and time are suitable reaction conditions for the coupling agent, for example, the reaction can be carried out at room temperature for 1-2 hours.

[0032] There is no special limitation on the dosage and specific composition of the titanate coupling agent, and those skilled in the art can adjust the dosage of the coupling agent according to the modified object and the specific type of coupling agent. For example, in some preferred embodiments, the dosage of the coupling agent is 0.5%-5% of the mass of the wool fiber.

[0033] In some preferred embodiments, the titanate coupling agent may include any one or more of ethyl tris(β-aminopropionate) titanium (EAT), ethyl amide triacetate titanium (EATT), bis(dihydroxyphenyl) diisobutyrate titanium, and titanium n-butoxide.

[0034] The second embodiment of the present invention provides the modified wool fiber obtained according to the first technical solution.

[0035] The third embodiment of the present invention provides a composite foam material, comprising the modified wool fiber of the second technical solution and an aqueous resin, wherein the mass ratio of the modified wool fiber to the aqueous resin is 1: (1-10); the aqueous resin comprises any one or more of aqueous polyurethane, polyvinyl alcohol resin, polyacrylic acid resin, polyvinyl acid resin, styrene-butadiene resin, etc.

[0036] The modified wool fiber in the embodiment of the present invention has a rough surface and more surface active sites, so that when it is compounded with the water-based resin, a physical and mechanical lock can be formed at the interface between the modified wool fiber and the water-based resin, thereby improving the mechanical properties of the polyurethane. At the same time, since the wool fiber treated with the enzyme contains a large number of voids inside, when it is compounded with the foaming material, the porosity of the foaming material can be significantly improved, and the flame retardant, heat insulating and thermal insulation properties of the foaming material can be improved.

[0037] The fourth embodiment of the present invention provides a method for preparing a composite foam material, that is, the method for preparing a composite foam material in the third embodiment, specifically comprising blending the modified wool fiber / combined modified wool fiber with an aqueous resin, stirring the mixture at a rate of 1000-5000 r / min for 5-30 min at room temperature for sufficient foaming, and drying.

[0038] There is no need to specifically limit the drying temperature and time, and those skilled in the art can adjust them adaptively according to the needs of the final product. For example, in some preferred embodiments, the drying temperature can be 60-105°C.

[0039] In order to make the technical solution of the present invention clearer, the preparation method, application and performance of the modified wool fiber are described in detail through multiple specific embodiments below.

[0040] Some of the substance information used in the specific embodiments of the present invention may be as follows:

[0041] Waste wool fiber, sourced from Xinji Baolong Technology Co., Ltd.;

[0042] Water-based polyurethane: model KT651G, manufacturer: Hefei Ketian Water-based Technology Co., Ltd.; but not limited to this.

[0043] The wool fibers used in the following specific embodiments can be prepared from wool waste (but not limited thereto), and the specific preparation method can be referred to as follows:

[0044] The waste wool is crushed using a pulverizer with a cooling device or a wind dispersing device, passed through a 40-mesh sieve, and the pretreated wool fibers are opened using a pulping machine (rotation speed is 2000 r / min) to obtain pretreated wool fibers.

[0045] Example 1

[0046] This embodiment provides a method for preparing modified wool fiber, comprising the following steps:

[0047] (1) Dissolve 50 g of cysteine ​​desulfurase in 10 L of Tris-HCl buffer (pH = 8). Take 1 kg of pretreated wool fiber and soak it in the treatment solution at 35 °C. After modification for 2 h, filter and wash three times to obtain enzyme-treated wool fiber.

[0048] (2) Take 30 g of ethyl tri(β-aminopropionic acid) titanium (EAT) with a purity of 90% and fully dissolve it in 1500 parts of water to prepare a coupling agent solution. Mix the coupling agent solution with the enzyme-treated wool fiber, stir at room temperature for 1 hour, filter, and wash the solid material with water. Repeat this process 3 times to remove the unreacted coupling agent. Then, dry the solid material at 80±2°C for 24 hours to obtain modified wool fiber.

[0049] Example 2

[0050] This example is based on the preparation method of Example 1, except that:

[0051] In step (1), the amount of cysteine ​​desulfurase used is 0.1% of the fiber mass.

[0052] Example 3

[0053] This example is based on the preparation method of Example 1, except that:

[0054] In step (1), the amount of cysteine ​​desulfurase used is 10% of the fiber mass.

[0055] Example 4

[0056] This example is based on the preparation method of Example 1, except that:

[0057] In step (2), the amount of chelated titanate coupling agent used is 0.5%.

[0058] Example 5

[0059] This example is based on the preparation method of Example 1, except that:

[0060] In step (2), the amount of the chelated titanate coupling agent used is 5%.

[0061] Example 6

[0062] This example is based on the preparation method of Example 1, except that:

[0063] In step (2), the chelated titanate coupling agent used is ethylamide triacetate titanate.

[0064] Comparative Example 1

[0065] This comparative example refers to the preparation method of Example 1, with the only difference being that only step (1) is performed without step (2), and thus the modified wool fiber treated with only enzyme is prepared.

[0066] Examples 7-15, Comparative Example 2

[0067] Examples 7-15 and Comparative Example 2 provide different composite foam materials and preparation methods thereof, and the raw material proportions are shown in Table 1 below.

[0068] Table 1 Raw material ratios of different composite foam materials

[0069] .

[0070] The preparation method of the composite foam material of Examples 7-15 and Comparative Example 2 comprises the following steps:

[0071] The modified wool fiber and the waterborne polyurethane foam material were blended in the above proportions, stirred at a rate of 3000 r / min at room temperature for 10 min, poured into a polytetrafluoroethylene mold, placed in an oven at 100±3°C, and taken out after drying to obtain a composite foam material.

[0072] Comparative Example 3

[0073] This comparative example refers to the preparation method of Example 8, except that the modified wool fiber of Example 8 is replaced by an equal amount of unmodified wool fiber.

[0074] Comparative Example 4

[0075] This comparative example refers to the preparation method of Example 8, with the only difference being that the modified wool fiber of Example 8 is replaced by an equal amount of wool fiber treated with only a titanate coupling agent but not an enzyme, that is, step (1) is omitted in Example 1, and step (2) is directly performed to obtain the modified wool fiber.

[0076] Experimental Example 1

[0077] In order to compare and illustrate the porosity of the composite foam materials of various embodiments of the present invention and comparative examples, the porosity of the materials of Examples 7-15 and Comparative Examples 2-4 was tested with reference to GB / T21650.1-2008 standard. The test results are shown in Table 2.

[0078] Table 2 Porosity test results of different composite foam materials

[0079] .

[0080] Experimental Example 2

[0081] In order to compare and illustrate the tensile strength of the composite foam materials of various embodiments of the present invention and comparative examples, the tensile properties of the materials of embodiments 8-15 and comparative examples 1-2 were tested with reference to ASTM D412 standard. The test results are shown in Table 3.

[0082] Table 3 Tensile strength test results of different composite foam materials

[0083] .

[0084] Experimental Example 3

[0085] In order to compare and illustrate the compressive strength of the modified waterborne polyurethane foam composite materials of the embodiments of the present invention and the comparative examples, the compression properties of the materials of embodiments 8-15 and comparative examples 1-2 were tested with reference to ASTM D1621 standard. The test results are shown in Table 4.

[0086] Table 4 Compressive strength test results of different composite foam materials

[0087] .

[0088] Experimental Example 4

[0089] In order to compare and illustrate the flame retardant properties of the composite foam materials of various embodiments of the present invention and comparative examples, the flame retardant properties of the materials of embodiments 8-15 and comparative examples 1-2 were tested with reference to ASTM D2863-77 standard. The test results are shown in Table 5.

[0090] Table 5 Flame retardant test results of different composite foam materials

[0091] .

[0092] Experimental Example 5

[0093] In order to compare and illustrate the thermal insulation performance of the composite foam materials of various embodiments of the present invention and comparative examples, the thermal insulation performance of the materials of embodiments 8-15 and comparative examples 1-2 was tested with reference to ISO22007-2 standard. The test results are shown in Table 6.

[0094] Table 6 Thermal conductivity test results of different composite foam materials

[0095] .

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A composite foam material, characterized in that: It comprises modified wool fiber and water-based resin, wherein the mass ratio of the modified wool fiber to the water-based resin is 1:(1-10); The water-based resin is water-based polyurethane; The preparation method of the modified wool fiber comprises the following steps: opening the pretreated wool fiber, performing enzyme treatment with cysteine ​​desulfurase, and washing the pretreated wool fiber to obtain the enzyme-treated wool fiber; mixing the enzyme-treated wool fiber with a titanate coupling agent solution to react, filtering, and drying to obtain the modified wool fiber.

2. The composite foam material according to claim 1, characterized in that: The mass of the cysteine ​​desulfurase is 0.1%-10% of the mass of the wool fiber.

3. The composite foam material according to claim 1, characterized in that: The enzyme treatment temperature is 20-55°C and the time is 0.5-2h.

4. The composite foam material according to claim 1, characterized in that: The mass of the titanate coupling agent is 0.5%-5% of the mass of the wool fiber.

5. The composite foam material according to claim 1 or 4, characterized in that: The titanate coupling agent comprises any one or more of ethyl tris(β-aminopropionate) titanium, ethylamide triacetate titanate, di(dihydroxyphenyl) diisobutyrate titanium, and n-butyrate titanium.

6. The composite foam material according to claim 1, characterized in that: The mixed reaction is carried out at room temperature for 1-2 hours.

7. The composite foam material according to claim 1, characterized in that: The pretreated wool fiber is obtained by crushing the wool fiber into 20-200 meshes.

8. The composite foam material according to claim 1, characterized in that: After the modified wool fiber is blended with the water-based resin, the mixture is stirred at a rate of 1000-5000 r / min for 5-30 min at room temperature to fully foam and then dried.