Solder alloys, solder balls, solder preforms, solder pastes and solder joints

By optimizing the alloy composition of Sn-Ag-Cu solder alloy, especially increasing Ag and micro-alloy structure, the problem of brazed joint fracture in harsh environments is solved, and a high-reliability brazing connection is achieved.

CN118043166BActive Publication Date: 2024-11-12SENJU METAL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280066205.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-29
Publication Date
2024-11-12
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

The existing Sn-3Ag-0.5Cu solder alloys are prone to fracture of the brazed joints in the face of severe temperature differences and physical external forces, and their wettability is insufficient, affecting the reliability of the connection.

Method used

By optimizing the content of Ag, Cu, Sb, In and Ni in the Sn-Ag-Cu solder alloy, controlling their alloy composition within a specific range, increasing the content of Ag to promote the solid phase transition from βSn to γSn to alleviate the stress and improve wettability and strength by fine-tuning the alloy structure and the alloy structure at the bonding interface.

Benefits of technology

It achieves excellent wettability and suppresses the fracture of the brazed joint, improves the reliability and strength of the brazed joint, and meets the long-term use needs in high and low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118043166B_ABST
    Figure CN118043166B_ABST
Patent Text Reader

Abstract

Provided are a solder alloy and a solder joint having excellent wettability, which suppresses the fracture of the solder joint and has high reliability. The solder alloy has an alloy composition of Ag: 1.0-3.7%, Cu: 0.4-0.8%, Sb: 0.50-2.90%, In: 5.00-10.00%, Ni: 0.01-0.06%, and the balance Sn.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to solder alloys, solder balls, solder preforms, solder pastes and solder joints used in various electronic devices. Background Art

[0002] In recent years, due to the high functionality of consumer electronic devices such as personal computers, the performance of electronic components mounted on substrates has improved dramatically. As electronic components become more high-performance, large currents are passed through them, so solder joints used in substrates of consumer electronic devices are sometimes exposed to high temperatures. In addition, when the substrate and electronic components are joined using soft soldering based on setp soldering, the solder joints are exposed to a high temperature of about 150°C. On the other hand, it is easy to imagine that consumer electronic devices are used in cold regions.

[0003] As applications where solder joints are exposed to harsh environments, in addition to consumer electronic components, automotive electronic devices or industrial electronic devices can be listed. The electronicization of automobiles is advancing, gradually migrating from gasoline vehicles to hybrid vehicles to electric vehicles. With this, substrates of automotive electronic devices are sometimes placed in locations such as engine rooms where they are exposed to high temperatures due to the expansion of their uses. On the other hand, when the engine is stopped, if it is in a cold area, it will be exposed to low temperatures of less than -40°C. Furthermore, depending on the use environment, physical external forces such as impacts may sometimes be applied to electronic equipment.

[0004] Industrial electronic devices are used in places where it is difficult for operators to work. Therefore, similarly to the substrates of vehicle-mounted electronic devices, the substrates of industrial electronic devices are likely to be exposed to environments with a sharp temperature difference or external forces may be applied to the electronic devices.

[0005] In addition, Sn-3Ag-0.5Cu solder alloy is widely used as an alloy for connecting substrates and electronic components. Although the application range of solder alloys is gradually expanding, with this, high connection reliability is gradually being required, such as in automotive applications, which does not cause cracks or deterioration in the solder joint even in harsh environments and long-term use.

[0006] However, if the electronic circuit is exposed to the temperature difference as described above, the difference in thermal expansion coefficient between the electronic component and the printed circuit board will cause stress to concentrate on the solder joint. In addition, when external force is applied to the electronic device, the stress will concentrate on the solder joint with a small cross-sectional area. Therefore, if the existing Sn-3Ag-0.5Cu solder alloy is used, there is a concern that the solder joint will break, and a solder alloy that suppresses this is sought.

[0007] For example, Patent Document 1 discloses an alloy composition in which Ni or the like can be contained in a Sn-Ag-Cu-Sb-In solder alloy as a solder alloy that suppresses deviation when forming a solder fillet in a through hole of a substrate, has excellent wettability and spreadability of molten solder, and has low crack progression due to thermal cycling. Comparative Example 6 of the same document discloses a solder alloy of 3.5 mass % Ag, 0.8 mass % Cu, 1.0 mass % Sb, 6.0 mass % In, 0.07 mass % Ni, and the remainder Sn.

[0008] Patent Document 2 discloses an alloy composition that can contain Sb, In, etc. as arbitrary elements in a Sn-Ag-Bi-Ni-Co solder alloy as a solder alloy with a small intermetallic compound structure, excellent crack resistance, suppressed pores and Cu leaching, and suppressed cracking after thermal cycling, thereby having excellent durability. Example 40 of the same document discloses a solder alloy of 3.0 mass % Ag, 0.5 mass % Cu, 1.5 mass % Sb, 4.3 mass % In, 0.05 mass % Ni, 0.5 mass % Bi, 0.005 mass % Co, and the balance Sn.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2019-063830

[0012] Patent Document 2: Japanese Patent Application Publication No. 2014-037005 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] However, the solder alloys described in Patent Documents 1 and 2 are designed mainly with an eye on thermal cycle characteristics as described above. If an electronic device is exposed to a thermal cycle, stress is applied to the solder joint due to the difference in thermal expansion coefficients between the substrate and the electronic components. On the other hand, it is believed that when vibration is applied to the on-board electronic circuit, the stress is applied in a different manner from the stress caused by the expansion and contraction of the printed substrate and electronic components generated during the thermal cycle. Thus, in order to avoid the fracture of the solder joint even when various stresses are applied to the solder joint due to the deterioration of the use environment caused by the high functionality and expansion of the use of electronic equipment in recent years, it is necessary to improve the strength of the solder alloy itself.

[0015] In addition, the fracture of the solder joint can be caused by the fracture of the solder alloy constituting the solder joint, and the fracture at the joint interface caused by the poor wettability of the solder alloy. Thus, in order to form a solder joint with higher reliability than before, it is necessary to re-examine the known alloy composition.

[0016] An object of the present invention is to provide a solder alloy, a solder ball, a solder preform, a solder paste, and a solder joint which are excellent in wettability, have cracking of the solder joint suppressed, and thus have high reliability.

[0017] Solutions for solving problems

[0018] The present inventors have studied alloy compositions that can relax various stresses in Sn-Ag-Cu solder alloys. It has been previously believed that solder alloys with large volume changes during hot and cold cycles will cause solder joints to break due to the difference in linear expansion coefficients with the substrate. However, when the volume change is small, the applied stress will be accumulated in the solder alloy in the form of strain energy, which may promote breakage.

[0019] First, the inventors of the present invention paid special attention to In, which causes volume changes in the solder alloy, in order to relax the stress applied during heating in a cold and hot cycle. In, depending on the content, promotes the solid phase transformation of βSn and γSn, thereby causing volume changes based on the solid phase transformation. Therefore, the inventors of the present invention studied solder alloys with increased In content as described in Patent Document 1.

[0020] However, if the volume change is large, the solder joint will break at the joint interface. Therefore, the present inventors have studied the contents of Cu, Sb and Ni in detail from the perspective of the wettability of the molten solder and the refinement of the alloy structure in the solder alloy and the alloy structure at the joint interface. Furthermore, the present inventors have paid attention to the fact that when the temperature of the solder joint rises during the hot and cold cycle, if a solid phase transition from βSn to γSn occurs immediately, the stress will be quickly relieved, and the content of Ag has also been studied in detail. As a result, the following insight was obtained: by using a solder alloy in which the contents of Ag, Cu, Sb, In and Ni as added elements are simultaneously within the specified range, the wettability is excellent and the breakage of the solder joint is suppressed, thereby completing the present invention.

[0021] The present invention obtained based on the above findings is as follows.

[0022] (1) A solder alloy characterized by having an alloy composition of, in mass %, 1.0 to 3.7% Ag, 0.4 to 0.8% Cu, 0.50 to 2.90% Sb, 5.00 to 10.00% In, 0.01 to 0.06% Ni, and the balance being Sn.

[0023] (2) The solder alloy according to (1) above, further comprising, in mass%, Co: 0.100% or less.

[0024] (3) The solder alloy according to (1) or (2) above, further comprising, in mass%, 5.0% or less of Bi.

[0025] (4) A solder alloy according to any one of (1) to (3), further comprising, in total, 0.1% by mass or less, at least one of Zr, Fe, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mn, Mo, Pt, Pd, Au, Al and Si.

[0026] (5) The solder alloy according to any one of (1) to (5) above, wherein the alloy composition satisfies the following formulas (1) and (2).

[0027] 132≤(In / Sb)×(Sn / Ag)≤450 (1)

[0028] 251≤In / (Cu×Sb×Ni)≤699 (2)

[0029] In the above formulas (1) and (2), In, Sb, Sn, Ag, Cu and Ni represent the contents (mass %) of the alloy composition.

[0030] (6) A solder ball comprising the solder alloy according to any one of (1) to (5) above.

[0031] (7) A preform solder formed from the solder alloy described in any one of (1) to (5) above.

[0032] (8) A solder paste comprising a solder powder formed of the solder alloy according to any one of (1) to (5) above.

[0033] (9) A solder joint comprising the solder alloy according to any one of (1) to (5) above. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a cross-sectional SEM photo of the solder alloy. Figure 1 (a) is Example 6, Figure 1 (b) is Comparative Example 3, Figure 1 (c) is Comparative Example 8. DETAILED DESCRIPTION

[0035] The present invention will be described in more detail below. In the present specification, "%" referring to the composition of the solder alloy means "mass %" unless otherwise specified.

[0036] 1. Solder alloy

[0037] (1) Ag: 1.0~3.7%

[0038] Ag reduces the temperature at which βSn transforms into γSn, thereby rapidly relieving strain energy when the temperature rises and suppressing the fracture of the solder joint. In addition, a network of Ag3Sn can be formed to improve the strength of the solder alloy itself. If the Ag content is less than 1.0%, the phase transition temperature from βSn to γSn will not drop, phase transition will not occur, and the fracture of the solder joint cannot be suppressed. In addition, a fine Ag3Sn network will not be formed, and the strength will be reduced. The lower limit of the Ag content is 1.0% or more, preferably 1.5% or more, and more preferably 2.0% or more. On the other hand, if the Ag content exceeds 3.7%, the coarse primary crystals of Ag3Sn will crystallize and the strength will deteriorate. The upper limit of the Ag content is 3.7% or less, preferably 3.0% or less, and more preferably 2.3% or less.

[0039] (2) Cu: 0.4-0.8%

[0040] Cu can improve the wettability of molten solder by suppressing the liquidus temperature. When the Cu content is less than 0.4% or exceeds 0.8%, the liquidus temperature will rise, the fluidity at the bonding temperature will decrease, and the wettability will deteriorate. In addition, if the Cu content exceeds 0.8%, a compound with Sn will precipitate, and the intermetallic compound formed at the bonding interface will become hard. The lower limit of the Cu content is 0.4% or more, preferably 0.5% or more. The upper limit of the Cu content is 0.8% or less, preferably 0.7% or less, and more preferably 0.6% or less.

[0041] (3) Sb: 0.50-2.90%

[0042] If Sb is added to a solder alloy containing a specified amount of In, fine InSb compounds will be crystallized, which can improve the strength of the solder alloy itself. In addition, the solid solubility limit of Sb to Sn changes in the use temperature range including room temperature, so Sb will be repeatedly dissolved and precipitated into Sn according to temperature changes. In addition, Sb forms a supersaturated solid solution in a high temperature domain, so the bulk strength of the solder alloy is improved based on solid solution strengthening. Accompanying this, the liquidus temperature is reduced, so wettability is improved.

[0043] If the Sb content is less than 0.50%, the improvement of bulk strength based on solid solution strengthening and dispersion precipitation strengthening cannot be achieved. In addition, the InSb compound will not become fine and the bulk strength will not be improved. The lower limit of the Sb content is 0.50% or more, preferably 0.70% or more, and more preferably 1.00% or more. On the other hand, if the Sb content exceeds 2.90%, the continuity of dispersion precipitation strengthening disappears due to the crystallization of coarse InSb compounds. The upper limit of the Sb content is 2.90% or less, preferably 2.50% or less, and more preferably 2.30% or less.

[0044] (4) In: 5.00~10.00%

[0045] When In reaches the phase transformation point due to temperature change, it will slowly transform βSn into γSn, thereby alleviating strain energy and suppressing the fracture of the brazed joint. In the past, it was believed that the brazed joint was prone to fracture when the volume change during the cold and hot cycle was large, but in the present invention, the alloy composition is deliberately adjusted in a way that the volume change becomes larger, thereby suppressing the breakage of the brazed joint compared to the existing solder alloy. If the In content is less than 5.0%, the solid phase transformation of the Sn phase will not occur. The lower limit of the In content is 5.0% or more, preferably 6.00% or more, and more preferably 7.50% or more. On the other hand, if the In content exceeds 10.00%, the liquidus temperature drops excessively, and the solid phase transformation of the Sn phase will not occur. The upper limit of the In content is 10.00% or less, preferably 9.00% or less.

[0046] (5) Ni: 0.01-0.06%

[0047] Ni will hinder the diffusion of Cu to Sn after soldering, inhibit the growth of intermetallic compounds precipitated at the joint interface, and also inhibit the coarsening of intermetallic compounds precipitated at the joint interface, thereby strengthening the joint interface. If the Ni content is less than 0.01%, strengthening of the joint interface cannot be achieved. The lower limit of the Ni content is 0.01% or more, preferably 0.02% or more, and more preferably 0.03% or more. On the other hand, if the Ni content exceeds 0.06%, wettability decreases due to the increase in liquidus temperature. The upper limit of the Ni content is 0.06% or less, preferably 0.05% or less, and more preferably 0.04% or less.

[0048] (6) Residue: Sn

[0049] The solder alloy of the present invention has a balance of Sn. It may contain inevitable impurities other than the aforementioned elements. Even if it contains inevitable impurities, it has no influence on the aforementioned effects.

[0050] (7) Co: 0.100% or less

[0051] Co is an arbitrary element that has the effect of inhibiting the growth of intermetallic compounds and making the alloy structure fine. The upper limit of the Co content is preferably 0.100% or less, more preferably 0.050% or less, and further preferably 0.010% or less. The lower limit of the Co content is not particularly limited, but from the viewpoint of achieving the refinement of the alloy structure, it is preferably 0.001% or more, more preferably 0.003% or more, further preferably 0.005% or more, further more preferably 0.006% or more, particularly preferably 0.007% or more, and most preferably 0.008% or more.

[0052] (8) Bi: 5.0% or less

[0053] Bi is an arbitrary element that dissolves in the Sn phase and can improve the strength of the solder alloy. In addition, if an appropriate amount is added, the solder alloy will not become brittle and sometimes maintain high strength. The upper limit of the Bi content is preferably 5.0% or less, more preferably 1.0% or less, and further preferably 0.3% or less. The lower limit of the Bi content is not particularly limited, and from the viewpoint of fully achieving solid solution strengthening, it only needs to be 0.1% or more.

[0054] (9) Any other element

[0055] In addition to the above, the solder alloy of the present invention may also contain at least one of Zr, Fe, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mn, Mo, Pt, Pd, Au, Al and Si in an amount of 0.1% or less in total. Even if it contains less than 0.1% of these elements, coarse compounds will not precipitate, and the above-mentioned effects of the present invention can be exerted. The total content of these elements is preferably less than 0.1%, more preferably less than 0.09%, and further preferably less than 0.05%. There is no particular limitation on the content of each element, but it is preferably 0.0003 to 0.02%. Among these, Fe, like Ni, can inhibit the growth of intermetallic compounds precipitated at the bonding interface by hindering the diffusion of Cu to Sn after soldering, and also inhibit the coarsening of intermetallic compounds precipitated at the bonding interface, thereby strengthening the bonding interface.

[0056] (10) Formula (1), Formula (2)

[0057] 132≤(In / Sb)×(Sn / Ag)≤450 (1)

[0058] 251≤In / (Cu×Sb×Ni)≤699 (2)

[0059] In the above formulas (1) and (2), In, Sb, Sn, Ag, Cu and Ni represent the contents (mass %) of the alloy composition.

[0060] The solder alloy of the present invention preferably satisfies the equations (1) and (2). If both equations are satisfied, the strength of the solder alloy itself is improved, and wettability can be improved by optimizing the liquidus temperature.

[0061] If the solder alloy of the present invention satisfies formula (1), Ag3Sn is densely crystallized and InSb is finely crystallized, thereby achieving a further improvement in bulk strength in a synergistic manner. In order to make each intermetallic compound dense and finely crystallized, it is desirable to contain the constituent elements of each intermetallic compound in a well-balanced manner. In addition, it is inferred that the amount of crystallization of the intermetallic compound is dispersed without being biased towards any one, thereby suppressing the coarsening of the intermetallic compound. The lower limit of formula (1) is preferably 132 or more, more preferably 150 or more, and particularly preferably 180 or more. The upper limit of (1) is preferably 450 or less, more preferably 430 or less, and further preferably 410 or less.

[0062] In addition, if the solder alloy of the present invention satisfies formula (2), the liquidus temperature can be adjusted to a more appropriate range. To this end, it is ideal to maintain a balanced content of In, which lowers the liquidus temperature when the content is high, and Cu, Sb and Ni, which increase the liquidus temperature when the content is high. In particular, Cu, Sb and Ni form intermetallic compounds with a higher melting point than Sn. Therefore, in order to optimize the liquidus temperature, it is expected to make a comprehensive adjustment together with the In content. The lower limit of formula (2) is preferably 251 or more, more preferably 300 or more, and particularly preferably 345 or more. The upper limit of formula (2) is preferably 699 or less, more preferably 600 or less, and further preferably 500 or less.

[0063] For the solder alloy of the present invention, as described above, in order to achieve the improvement of mechanical properties, it is expected that Ag3Sn is densely crystallized and InSb is finely crystallized. The evaluation of density and fineness is usually evaluated by the average grain size. However, even if there is one coarse compound, it is possible to deteriorate the mechanical properties of the solder alloy. Therefore, in the present invention, the maximum grain diameter of these compounds is focused on. If the maximum grain diameter is small, it can be evaluated as a dense and fine structure. In Ag3Sn, the most suitable particle size is preferably 5 to 15 μm, more preferably 5 to 10 μm, and it can also exceed 10 μm and be less than 15 μm. In InSb, the maximum grain diameter is preferably less than 7 μm, more preferably less than 5 μm, and further preferably less than 1.8 μm.

[0064] 2. Solder balls

[0065] The solder alloy of the present invention can be used as a solder ball. The solder ball of the present invention is used to form electrodes of semiconductor packages such as BGA (ball grid array package) and bumps of substrates. The diameter of the solder ball of the present invention is preferably in the range of 1 to 1000 μm. The solder ball can be manufactured according to a general solder ball manufacturing method.

[0066] 3. Preformed solder

[0067] The shape of the preformed solder of the present invention is not particularly limited, and can be used in the form of a plate, ring, cylinder, spiral ribbon, square, disk, washer, chip, wire, etc. The preformed solder has a higher melting point than the solder alloy, and can contain high melting point metal particles (such as Ni particles, Cu particles, and alloy powders with Ni and Cu as main components) that are easily infiltrated into the molten solder.

[0068] 4. Solder paste

[0069] The solder alloy of the present invention can be used as a solder paste. A solder paste is a paste-like substance obtained by mixing solder alloy powder with a small amount of flux. The solder alloy of the present invention can be used as a solder paste in the mounting of electronic components on a printed circuit board based on a reflow soldering method. The flux used in the solder paste can be any of a water-soluble flux and a non-water-soluble flux. Typically, a rosin-based flux that is a non-water-soluble flux based on a rosin base is used.

[0070] 5. Brazing joints

[0071] The solder joint of the present invention connects the IC chip in the semiconductor package to its substrate (interposer), or connects the semiconductor package to the printed circuit board. That is, the solder joint of the present invention is called the connecting portion of the electrode, and can be formed using general soldering conditions.

[0072] The bonding method using the solder alloy of the present invention can be carried out according to conventional methods such as step soldering based on the reflow method. The heating temperature can be appropriately adjusted according to the heat resistance of the chip and the liquidus temperature of the solder alloy. Other bonding conditions can be appropriately adjusted according to the alloy composition of the solder alloy.

[0073] Example

[0074] A solder alloy composed of the alloy compositions shown in Tables 1 and 2 was prepared, and as evaluation 1, the liquidus temperature was measured, as evaluation 2, the compactness of Ag3Sn was evaluated, as evaluation 3, the miniaturization of InSb was evaluated, as evaluation 4, the solid phase transformation of the Sn phase was evaluated, and as evaluation 5, the uniform miniaturization of the bonding interface was evaluated.

[0075] Evaluation 1: Liquidus temperature

[0076] Each solder alloy in Table 1 was prepared, and the liquidus temperature of the solder alloy was measured. The liquidus temperature was measured by the same DSC method as the solidus temperature measurement method of JIS Z3198-1. When the liquidus temperature was 200 to 215°C, it was evaluated as "0", when it exceeded 215°C, it was evaluated as "×", and when it was lower than 200°C, it was also recorded as "×".

[0077] Evaluation 2, 3: Compactness of Ag3Sn and miniaturization of InSb

[0078] A solder alloy composed of the alloy composition shown in Table 1 was injected into a specified mold, the obtained solder alloy was molded with resin and polished, and the part where the solder alloy was polished about half was photographed with FE-SEM at a magnification of 1000 times. The compactness of Ag3Sn and the miniaturization of InSb were evaluated by cross-sectional observation and EDS-based mapping composition analysis. Each compound was identified by mapping composition analysis, and the largest grain was selected by visual inspection. For the grain, two parallel tangents were drawn in a way that the interval was the largest, and the interval was taken as the maximum grain diameter. When the maximum grain diameter of Ag3Sn is 5μm or more and 10μm or less, it is recorded as "◎", when it is more than 10μm and less than 15μm, it is recorded as "○", and when it is less than 5μm and when it is more than 15μm, it is recorded as "×". In addition, when the maximum crystal grain size of InSb is 1.8 μm or less, it is recorded as “◎”, when it exceeds 1.8 μm and is 7 μm or less, it is recorded as “○”, and when it exceeds 7 μm, it is recorded as “×”.

[0079] Evaluation 4: Solid-state phase transition of Sn phase

[0080] Prepared from the solder alloys shown in Tables 1 to 3 Using a constant temperature bath, the solder ball is exposed to The solder balls were evaluated under a thermal cycle environment with 200 cycles of 37°C and 40°C conditions and in an environment where a solid phase transition of the Sn phase occurs. Afterwards, the sphericity of the solder balls taken out of the thermostatic chamber was evaluated. The sphericity was measured using a CNC image measurement system. The devices were ULTRA QUICK VISION and ULTRA QV350-PRO manufactured by Mitutoyo. If the sphericity was less than 0.95, it was evaluated as "◎", if the sphericity was greater than 0.95 and less than 0.99, it was evaluated as "0", and if the sphericity was greater than 0.99, it was evaluated as "×".

[0081] Evaluation 5: Uniform refinement of the bonding interface

[0082] Prepared from the solder alloys shown in Table 1 A solder ball is placed on a Cu bump and then reflowed at 245°C to make a solder bump. The thickness of the intermetallic compound (IMC) is measured by taking a cross-sectional SEM photograph of the cross-section of the bonding interface between the solder bump and the Cu bump to evaluate the uniform miniaturization of the bonding interface. When the bonding interface is uniform and becomes fine, the intermetallic compound layer becomes thinner. Therefore, in Evaluation 5, the thickness of the intermetallic compound is used to evaluate the uniform miniaturization. The cross-sectional SEM photograph is analyzed using image analysis software (manufactured by Seika Industry Co., Ltd.: Scandium) to measure the thickness of the intermetallic compound layer. If the thickness of the intermetallic compound is less than 1.5μm, it is evaluated as "◎", if it exceeds 1.5μm and is less than 2.5μm, it is evaluated as "0", and if it exceeds 2.5μm, it is evaluated as "×".

[0083] The evaluation results are shown in Tables 1 to 3.

[0084] [Table 1]

[0085]

[0086] [Table 2]

[0087]

[0088] [Table 3]

[0089]

[0090] Tables 1 to 3 show that the constituent elements of Examples 1 to 48 are all appropriate, and therefore the liquidus temperature shows a temperature within the specified range. In addition, Ag3Sn is dense and InSb is fine, and a solid phase transition from βSn to γSn is confirmed, and the structure of the bonding interface becomes uniform and fine. In particular, Examples 3 to 8, 14, 15, and 18 to 48, which are confirmed to satisfy equations (1) and (2), show excellent results in all evaluations.

[0091] On the other hand, since the Ag content in Comparative Example 1 is small and In is not contained, Ag3Sn is not dense enough to improve the bulk strength, and no solid phase transformation of the Sn phase can be confirmed.

[0092] The Ag content of Comparative Examples 2 and 3 was not appropriate, and therefore, Ag3Sn was not densified to such an extent that the bulk strength would be improved.

[0093] Comparative Examples 4 to 6 had inappropriate Cu contents as described below, and therefore did not reach the liquidus temperature at which excellent wettability was exhibited.

[0094] The Sb contents of Comparative Examples 7 and 8 were not appropriate, and therefore, InSb was not finely divided to such an extent that the bulk strength would be improved.

[0095] Since the In content of Comparative Examples 9 to 11 was not appropriate, the solid phase transition of the Sn phase could not be confirmed. In addition, since Comparative Example 11 did not contain Sb, the InSb compound did not precipitate.

[0096] Comparative Examples 12 and 13 have low Ni contents, so uniform refinement of the bonding interface cannot be confirmed. In addition, since Comparative Example 12 does not contain Sb, the InSb compound does not precipitate.

[0097] Since the Ni content in Comparative Example 14 was high, the liquidus temperature at which excellent wettability was exhibited was not reached.

[0098] These results are explained using the accompanying drawings. Figure 1 This is a cross-sectional SEM photo of the solder alloy. Figure 1 (a) is Example 6, Figure 1 (b) is Comparative Example 3, Figure 1 (c) is Comparative Example 8. Figure 1 The grain size of the Ag3Sn shown in (b) was measured in the portion surrounded by the dotted line. Figure 1 It is clear that in Example 6, Ag3Sn is less than 10 μm and is densely crystallized, and InSb is finely crystallized. It is also known that the intermetallic compound precipitated at the bonding interface is uniform and fine, and therefore thin. On the other hand, it is known that the Ag3Sn of Comparative Example 3 is coarse. In addition, it is known that the InSb of Comparative Example 8 is coarse.

Claims

1. A solder alloy, characterized in that: The present invention has an alloy composition of Ag: 1.0-3.7%, Cu: 0.4-0.8%, Sb: 0.50-2.90%, In: 5.00-10.00%, Ni: 0.01-0.06%, and the balance Sn, wherein the alloy composition satisfies the following formulas (1) and (2), 132≤(In / Sb)×(Sn / Ag)≤450 (1) 251≤In / (Cu×Sb×Ni)≤699 (2) In the above formula (1) and formula (2), In, Sb, Sn, Ag, Cu and Ni represent the contents of the above alloy composition in mass %. 2 . The solder alloy according to claim 1 , further comprising, by mass%, Co: 0.100% or less. 3 . The solder alloy according to claim 1 , further comprising, by mass%, 1.0% or less of Bi.

4. The solder alloy according to claim 1 or 2, further comprising, in terms of mass %, a total of 0.1% or less of at least one of Zr, Fe, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mn, Mo, Pt, Pd, Au, Al and Si.

5. The solder alloy according to claim 1 or 2, further comprising, by mass%, Bi: 5.0% or less, and a total of 0.1% or less of at least one of Zr, Ge, Ga, As, Pb, Mg, Cr, Ti, Mn, Mo, Pt, Pd and Si. 6 . A solder ball formed of the solder alloy according to claim 1 . 7 . A solder preform, comprising the solder alloy according to claim 1 . 8 . A solder paste comprising a solder powder formed of the solder alloy according to claim 1 . 9 . A solder joint comprising the solder alloy according to claim 1 .