A kind of wear-resistant polyester resin powder coating and preparation method thereof

By synthesizing hyperbranched polyester step by step and adding wear-resistant fillers, combined with the electrostatic spraying method, the problem that existing powder coatings cannot meet the requirements for high wear-resistant coatings is solved, and the wear-resistant performance and compactness of the coating are significantly improved. .

CN118048107BActive Publication Date: 2024-10-18GUANGDONG JINGAOLI NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410180035.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-18
Publication Date
2024-10-18
Estimated Expiration
2044-02-18

AI Technical Summary

Technical Problem

Existing powder coatings cannot meet the requirements for highly wear-resistant coatings and are limited by the resin's glass transition temperature and solvent-free operating viscosity.

Method used

Hyperbranched polyester is synthesized step by step, and the tightness and wear resistance of the coating are improved by adding wear-resistant fillers and oxidized polyethylene wax, combined with electrostatic spraying.

Benefits of technology

The narrow molecular weight distribution range of polyester is achieved, the consistency and wear resistance of the coating are improved, and the compactness of the coating is enhanced, thereby significantly improving the wear resistance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004703459690000021
    Figure BDA0004703459690000021
  • Figure BDA0004703459690000081
    Figure BDA0004703459690000081
  • Figure BDA0004703459690000091
    Figure BDA0004703459690000091
Patent Text Reader

Abstract

The invention discloses a wear-resistant polyester resin powder coating and a preparation method thereof, and belongs to the technical field of coatings. The preparation of polyester comprises the following steps: taking 2,2-dimethylolbutanol, 2,2-dimethylolpropionic acid, and p-toluenesulfonic acid, placing them in a reactor, mixing and stirring, reacting, and reacting under reduced pressure to obtain material A; adding 2,2-dimethylolpropionic acid and p-toluenesulfonic acid, reacting, and reacting under reduced pressure to obtain material B; adding 2,2-dimethylolpropionic acid and p-toluenesulfonic acid, reacting, discharging, grinding, and sieving to obtain the polyester; the preparation of wear-resistant polyester resin powder coating comprises the following steps: taking polyester, wear-resistant filler, triglycidyl isocyanurate, Digo 410 leveling agent, diphenyl ethyl ketone, coupling agent RC201, and oxidized polyethylene wax, mixing and crushing, adding them to a twin-screw extruder, mixing, extruding, cooling, crushing, and sieving to obtain the wear-resistant polyester resin powder coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a wear-resistant polyester resin powder coating and a preparation method thereof. Background Art

[0002] Powder coating is a new type of solid powder coating without solvent, which has the characteristics of no solvent, no pollution, recyclable, environmental protection, energy saving and high mechanical strength of coating film. However, due to the limitations of resin glass transition temperature and solvent-free operating viscosity, the existing powder coating cannot meet the requirements for high wear-resistant coating. Summary of the invention

[0003] The invention discloses a wear-resistant polyester resin powder coating and a preparation method thereof, and belongs to the technical field of coatings. The preparation of polyester comprises the following steps: 2,2-dimethylolbutanol, 2,2-dimethylolpropionic acid and p-toluenesulfonic acid are placed in a reaction kettle for mixing and stirring, reacting, and reacting under reduced pressure to obtain material A; 2,2-dimethylolpropionic acid and p-toluenesulfonic acid are added, reacting, and reacting under reduced pressure to obtain material B; 2,2-dimethylolpropionic acid and p-toluenesulfonic acid are added, reacting, discharging, grinding, and sieving to obtain the polyester; the preparation of wear-resistant polyester resin powder coating comprises the following steps: polyester, wear-resistant filler, triglycidyl isocyanurate, Digo 410 leveling agent, diphenyl ethyl ketone, coupling agent RC201, and oxidized polyethylene wax are mixed and crushed, added to a twin-screw extruder for mixing, extruding, cooling, crushing, and sieving to obtain the wear-resistant polyester resin powder coating.

[0004] The technical problem to be solved by the present invention is to produce a polyester resin powder coating with excellent wear resistance.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A wear-resistant polyester resin powder coating, comprising the following raw materials in parts by weight:

[0007]

[0008] As a preferred technical solution of the present invention, the preparation of the polyester comprises the following steps:

[0009] S1, 2,2-dimethylolbutanol, 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were placed in a reaction kettle, stirred for 1-2 hours in a nitrogen atmosphere, reacted at 150-160° C. and normal pressure for 2-3 hours, and then the pressure in the reaction kettle was adjusted to 1-1.2 kPa and the reaction was continued for 2-3 hours to obtain material A;

[0010] S2, continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material A, stir for 1-2 hours in a nitrogen atmosphere, react at 150-160 ° C. under normal pressure for 2-3 hours, and then adjust the pressure in the reactor to 1-1.2 kPa and continue to react for 2-3 hours to obtain material B;

[0011] S3. Continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material B, stir for 1-2 hours in a nitrogen atmosphere, react at 150-160 ° C. under normal pressure for 2-3 hours, then adjust the pressure in the reactor to 1-1.2 kPa and continue to react for 2-3 hours, cool the material, grind it, and pass it through a 200-mesh sieve to obtain the polyester.

[0012] As a preferred technical solution of the present invention, the mass ratio of 2,2-dihydroxymethylbutanol in step S1, 2,2-dihydroxymethylpropionic acid in step S1, p-toluenesulfonic acid in step S1, 2,2-dihydroxymethylpropionic acid in step S2, p-toluenesulfonic acid in step S2, 2,2-dihydroxymethylpropionic acid in step S3, and p-toluenesulfonic acid in step S3 is 1.2-1.5: 0.3-0.4: 0.036-0.046: 0.33-0.42: 0.036-0.046: 0.28-0.36: 0.036-0.046.

[0013] As a preferred technical solution of the present invention, the preparation of the wear-resistant filler comprises the following steps:

[0014] Take anhydrous ethanol, ammonia water and deionized water, mix them, stir for 15-25 minutes, add silica sol, stir for 20-30 minutes, add ethyl orthosilicate and heptadecafluorodecyltrimethoxysilane, stir for 24-32 hours, dry in an oven at 80° C. for 8-10 hours, grind, and pass through a 300-mesh sieve to obtain the wear-resistant filler.

[0015] As a preferred technical solution of the present invention, the dosage ratio of anhydrous ethanol, ammonia water, deionized water, silica sol, ethyl orthosilicate, and heptadecafluorodecyltrimethoxysilane is 80-100mL: 4-6mL: 8-10mL: 1-3g: 0.6-0.8mL: 0.5-0.6mL.

[0016] As a preferred technical solution of the present invention, the mass fraction of the ammonia water is 25-28%.

[0017] As a preferred technical solution of the present invention, the concentration of silicon dioxide in the silica sol is 15%.

[0018] A method for preparing a wear-resistant polyester resin powder coating, the preparation of the wear-resistant polyester resin powder coating comprising the following steps:

[0019] A1, taking polyester, wear-resistant filler, triglycidyl isocyanurate, Digo 410 leveling agent, dibenzoyl ketone, coupling agent RC201, and oxidized polyethylene wax, mixing and grinding them in a high-speed grinder to obtain a mixed material;

[0020] A2, open the twin-screw extruder, raise the temperature to 105-115° C., add the mixed material into the twin-screw extruder and mix for 30-40 minutes, extrude, cool, crush, and pass through a 140-mesh sieve to obtain the wear-resistant polyester resin powder coating.

[0021] A method for using a wear-resistant polyester resin powder coating, wherein the wear-resistant polyester resin powder coating is transported to a spray gun via an airflow, and the wear-resistant polyester resin powder coating is sprayed onto a surface of an object to be coated by a high-voltage electrostatic spraying method, and a coating is formed after curing;

[0022] The spraying conditions are as follows: electrostatic high voltage 50-60 kV, current 60-65 A, and spraying gas pressure 0.4-0.5 MPa.

[0023] Beneficial effects of the present invention:

[0024] The wear-resistant polyester resin powder coating and preparation method thereof disclosed in the present invention uses a hyperbranched polyester synthesized in steps, and the obtained polyester has a narrow molecular weight distribution range, so that it has good consistency and stability, and improves the wear resistance of the coating;

[0025] Furthermore, the wear resistance of the coating is improved by adding wear-resistant fillers;

[0026] Furthermore, since the coating is obtained by electrostatic spraying, a large number of pores are generated inside the coating. By adding oxidized polyethylene wax and cooling and precipitating it to fill the pores, the compactness of the coating is increased, thereby improving its wear resistance. DETAILED DESCRIPTION

[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0028] Example 1

[0029] A method for preparing a wear-resistant polyester resin powder coating comprises the following steps:

[0030] A1, 50 parts by mass of polyester, 20 parts by mass of wear-resistant filler, 5 parts by mass of triglycidyl isocyanurate, 0.25 parts by mass of Digo 410 leveling agent, 0.3 parts by mass of benzoyl ketone, 0.2 parts by mass of coupling agent RC201, and 8 parts by mass of oxidized polyethylene wax were mixed and crushed in a high-speed pulverizer to obtain a mixed material;

[0031] A2, open the twin-screw extruder, heat it to 105 ° C, add the mixed material into the twin-screw extruder and mix for 30 minutes, extrude, cool, crush, and pass through a 140-mesh sieve to obtain the wear-resistant polyester resin powder coating.

[0032] The preparation of the polyester comprises the following steps:

[0033] S1, 2,2-dimethylolbutanol, 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were placed in a reaction kettle, stirred for 1 hour in a nitrogen atmosphere, reacted at 150° C. and normal pressure for 2 hours, and then the pressure in the reaction kettle was adjusted to 1 kPa and the reaction was continued for 2 hours to obtain material A;

[0034] S2, continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material A, stir for 1 hour in a nitrogen atmosphere, react at 150 ° C. under normal pressure for 2 hours, then adjust the pressure in the reactor to 1 kPa and continue to react for 2 hours to obtain material B;

[0035] S3. Continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material B, stir for 1 hour in a nitrogen atmosphere, react at 150° C. and normal pressure for 2 hours, then adjust the pressure in the reactor to 1 kPa and continue to react for 2 hours, cool the material, grind it, and pass it through a 200-mesh sieve to obtain the polyester.

[0036] The mass ratio of 2,2-dihydroxymethylbutanol in step S1, 2,2-dihydroxymethylpropionic acid in step S1, p-toluenesulfonic acid in step S1, 2,2-dihydroxymethylpropionic acid in step S2, p-toluenesulfonic acid in step S2, 2,2-dihydroxymethylpropionic acid in step S3, and p-toluenesulfonic acid in step S3 is 1.2:0.3:0.036:0.33:0.036:0.28:0.036.

[0037] The preparation of the wear-resistant filler comprises the following steps:

[0038] Take anhydrous ethanol, ammonia water and deionized water, mix them, stir for 15 minutes, add silica sol, stir for 20 minutes, add tetraethyl orthosilicate and heptadecafluorodecyltrimethoxysilane, stir for 24 hours, dry in an oven at 80°C for 8 hours, grind, and pass through a 300-mesh sieve to obtain the wear-resistant filler; the dosage ratio of the anhydrous ethanol, ammonia water, deionized water, silica sol, tetraethyl orthosilicate and heptadecafluorodecyltrimethoxysilane is 80mL: 4mL: 8mL: 1g: 0.6mL: 0.5mL; the mass fraction of the ammonia water is 25%; the concentration of silicon dioxide in the silica sol is 15%.

[0039] Example 2

[0040] A method for preparing a wear-resistant polyester resin powder coating comprises the following steps:

[0041] A1, 60 parts by mass of polyester, 25 parts by mass of wear-resistant filler, 6 parts by mass of triglycidyl isocyanurate, 0.4 parts by mass of Digo 410 leveling agent, 0.4 parts by mass of benzoyl ketone, 0.3 parts by mass of coupling agent RC201, and 10 parts by mass of oxidized polyethylene wax were mixed and crushed in a high-speed pulverizer to obtain a mixed material;

[0042] A2, open the twin-screw extruder, heat it to 110° C., add the mixed material into the twin-screw extruder and mix for 35 minutes, extrude, cool, crush, and pass through a 140-mesh sieve to obtain the wear-resistant polyester resin powder coating.

[0043] The preparation of the polyester comprises the following steps:

[0044] S1, 2,2-dimethylolbutanol, 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were placed in a reactor and mixed, stirred for 1.5 h in a nitrogen atmosphere, reacted at 155 ° C. and normal pressure for 2.5 h, and then the pressure in the reactor was adjusted to 1.1 kPa and the reaction was continued for 2.5 h to obtain material A;

[0045] S2, continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material A, stir for 1.5 hours in a nitrogen atmosphere, react at 155 ° C. at normal pressure for 2.5 hours, and then adjust the pressure in the reactor to 1.1 kPa and continue to react for 2.5 hours to obtain material B;

[0046] S3. Continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material B, stir for 1.5 hours in a nitrogen atmosphere, react at 155° C. and normal pressure for 2.5 hours, then adjust the pressure in the reactor to 1.1 kPa and continue to react for 2.5 hours, cool the material, grind it, and pass it through a 200-mesh sieve to obtain the polyester.

[0047] The mass ratio of 2,2-dihydroxymethylbutanol in step S1, 2,2-dihydroxymethylpropionic acid in step S1, p-toluenesulfonic acid in step S1, 2,2-dihydroxymethylpropionic acid in step S2, p-toluenesulfonic acid in step S2, 2,2-dihydroxymethylpropionic acid in step S3, and p-toluenesulfonic acid in step S3 is 1.35:0.35:0.04:0.38:0.04:0.32:0.04.

[0048] The preparation of the wear-resistant filler comprises the following steps:

[0049] Take anhydrous ethanol, ammonia water and deionized water, mix them, stir for 20 minutes, add silica sol, stir for 25 minutes, add tetraethyl orthosilicate and heptadecafluorodecyltrimethoxysilane, stir for 28 hours, dry in an oven at 80°C for 9 hours, grind, and pass through a 300-mesh sieve to obtain the wear-resistant filler; the dosage ratio of anhydrous ethanol, ammonia water, deionized water, silica sol, tetraethyl orthosilicate and heptadecafluorodecyltrimethoxysilane is 90mL: 5mL: 9mL: 2g: 0.7mL: 0.55mL; the mass fraction of the ammonia water is 26%; the concentration of silicon dioxide in the silica sol is 15%.

[0050] Example 3

[0051] A method for preparing a wear-resistant polyester resin powder coating comprises the following steps:

[0052] A1, 65 parts by mass of polyester, 30 parts by mass of wear-resistant filler, 8 parts by mass of triglycidyl isocyanurate, 0.5 parts by mass of Digo 410 leveling agent, 0.5 parts by mass of benzoyl ketone, 0.4 parts by mass of coupling agent RC201, and 13 parts by mass of oxidized polyethylene wax were mixed and crushed in a high-speed pulverizer to obtain a mixed material;

[0053] A2, open the twin-screw extruder, heat it to 115 ° C, add the mixed material into the twin-screw extruder and mix for 40 minutes, extrude, cool, crush, and pass through a 140-mesh screen to obtain the wear-resistant polyester resin powder coating.

[0054] The preparation of the polyester comprises the following steps:

[0055] S1, 2,2-dihydroxymethylbutanol, 2,2-dihydroxymethylpropionic acid and p-toluenesulfonic acid were placed in a reaction kettle, stirred for 2 hours in a nitrogen atmosphere, reacted at 160° C. and normal pressure for 3 hours, and then the pressure in the reaction kettle was adjusted to 1.2 kPa and the reaction was continued for 3 hours to obtain material A;

[0056] S2, continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material A, stir for 2 hours in a nitrogen atmosphere, react at 160 ° C. under normal pressure for 3 hours, and then adjust the pressure in the reactor to 1.2 kPa and continue to react for 3 hours to obtain material B;

[0057] S3. Continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material B, stir for 2 hours in a nitrogen atmosphere, react at 160° C. and normal pressure for 3 hours, then adjust the pressure in the reactor to 1.2 kPa and continue to react for 3 hours, cool the material, grind it, and pass it through a 200-mesh sieve to obtain the polyester.

[0058] The mass ratio of 2,2-dihydroxymethylbutanol in step S1, 2,2-dihydroxymethylpropionic acid in step S1, p-toluenesulfonic acid in step S1, 2,2-dihydroxymethylpropionic acid in step S2, p-toluenesulfonic acid in step S2, 2,2-dihydroxymethylpropionic acid in step S3, and p-toluenesulfonic acid in step S3 is 1.5:0.4:0.046:0.42:0.046:0.36:0.046.

[0059] The preparation of the wear-resistant filler comprises the following steps:

[0060] Take anhydrous ethanol, ammonia water and deionized water, mix them, stir for 25 minutes, add silica sol, stir for 30 minutes, add tetraethyl orthosilicate and heptadecafluorodecyltrimethoxysilane, stir for 32 hours, dry in an oven at 80°C for 10 hours, grind, and pass through a 300-mesh sieve to obtain the wear-resistant filler; the dosage ratio of the anhydrous ethanol, ammonia water, deionized water, silica sol, tetraethyl orthosilicate and heptadecafluorodecyltrimethoxysilane is 100mL: 6mL: 10mL: 3g: 0.8mL: 0.6mL; the mass fraction of the ammonia water is 28%; the concentration of silicon dioxide in the silica sol is 15%.

[0061] Comparative Example 1

[0062] The difference from Example 3 is that no oxidized polyethylene wax is added, and the other operations and steps remain unchanged.

[0063] Comparative Example 2

[0064] The difference from Example 3 is that no wear-resistant filler is added, and the other operations and steps remain unchanged.

[0065] Comparative Example 3

[0066] The difference from Example 3 is that the preparation of the polyester includes the following steps: taking 2,2-dihydroxymethylbutanol, 2,2-dihydroxymethylpropionic acid, and p-toluenesulfonic acid into a reactor and mixing them, stirring them in a nitrogen atmosphere for 6 hours, reacting them at 160°C and normal pressure for 9 hours, then adjusting the air pressure in the reactor to 1.2 kPa and continuing the reaction for 9 hours, cooling the material, grinding it, and passing it through a 200-mesh sieve to obtain the polyester; the mass ratio of the 2,2-dihydroxymethylbutanol, 2,2-dihydroxymethylpropionic acid, and p-toluenesulfonic acid is 1.5:1.18:0.138.

[0067] Performance Testing

[0068] Conduct coating wear resistance test according to standard GB / T 1768-2006;

[0069] The powder coatings prepared in Examples 1-3 and Comparative Examples 1-3 were respectively transported to a spray gun via an airflow, and the powder coatings were sprayed onto the surface of the coating sample by a high-voltage electrostatic spraying method to form a coating with a thickness of 10 μm; the spraying conditions were an electrostatic high voltage of 60 kV, a current of 65 A, and a spraying air pressure of 0.5 MPa; and then a wear resistance test was performed according to the above standards. The test results are shown in Table 1 below.

[0070] Table 1

[0071]

[0072]

[0073] As shown in Table 1, the coatings obtained by the powder coatings prepared in Examples 1-3 have excellent wear resistance; the coatings obtained by the powder coatings prepared in Comparative Examples 1-3 have poor wear resistance;

[0074] This is because the powder coating of Comparative Example 1 did not add oxidized polyethylene wax to fill the internal pores during the preparation process, resulting in reduced wear resistance of the coating; the powder coating of Comparative Example 2 did not add wear-resistant fillers with enhanced wear resistance of the coating during the preparation process, resulting in reduced wear resistance of the coating; the powder coating of Comparative Example 3 synthesized polyester in one step during the preparation process, resulting in a wider molecular weight distribution range, and the obtained polyester product had poor consistency and was unstable, resulting in reduced wear resistance of the coating.

[0075] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A wear-resistant polyester resin powder coating, It is characterized in that The wear-resistant polyester resin powder coating is composed of the following raw materials in parts by weight: Polyester 50-65 parts by mass Wear-resistant filler 20-30 parts by mass 5-8 parts by mass of triglycidyl isocyanurate Digo 410 leveling agent 0.25-0.5 mass parts 0.3-0.5 mass parts of benzoyl ketone Coupling agent RC201 0.2-0.4 parts by mass 8-13 parts by weight of oxidized polyethylene wax; The preparation of the polyester comprises the following steps: S1, 2,2-dimethylolbutanol, 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were placed in a reaction kettle, mixed, stirred in a nitrogen atmosphere, reacted at 150-160° C. under normal pressure, and the pressure was reduced to continue the reaction to obtain material A; S2, continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material A, stir in a nitrogen atmosphere, react at 150-160 ° C. under normal pressure, and continue to react under reduced pressure to obtain material B; S3, continue to add 2,2-dimethylolpropionic acid and p-toluenesulfonic acid to the reactor containing the material B, stir in a nitrogen atmosphere, react at 150-160° C. under normal pressure, continue to react under reduced pressure, cool the material, grind, and sieve to obtain the polyester; The mass ratio of 2,2-dimethylolbutanol in step S1, 2,2-dimethylolpropionic acid in step S1, p-toluenesulfonic acid in step S1, 2,2-dimethylolpropionic acid in step S2, p-toluenesulfonic acid in step S2, 2,2-dimethylolpropionic acid in step S3, and p-toluenesulfonic acid in step S3 is 1.2-1.5: 0.3-0.4: 0.036-0.046: 0.33-0.42: 0.036-0.046: 0.28-0.36: 0.036-0.046; The preparation of the wear-resistant filler comprises the following steps: Take anhydrous ethanol, ammonia water and deionized water, mix them, stir, add silica sol, stir, add ethyl orthosilicate and heptadecafluorodecyltrimethoxysilane, stir, dry, grind and sieve to obtain the wear-resistant filler; The dosage ratio of the anhydrous ethanol, ammonia water, deionized water, silica sol, ethyl orthosilicate and heptadecafluorodecyltrimethoxysilane is 80-100 mL: 4-6 mL: 8-10 mL: 1-3 g: 0.6-0.8 mL: 0.5-0.6 mL.

2. A wear-resistant polyester resin powder coating according to claim 1, It is characterized in that The mass fraction of the ammonia water is 25-28%.

3. The wear-resistant polyester resin powder coating according to claim 1, It is characterized in that The concentration of silicon dioxide in the silica sol is 15%.

4. A method for preparing the wear-resistant polyester resin powder coating according to any one of claims 1 to 3, It is characterized in that The preparation of the wear-resistant polyester resin powder coating comprises the following steps: A1, taking polyester, wear-resistant filler, triglycidyl isocyanurate, Digo 410 leveling agent, benzoyl ketone, coupling agent RC201, and oxidized polyethylene wax, mixing and grinding to obtain a mixed material; A2. Turn on the twin-screw extruder, raise the temperature to 105-115° C., add the mixed material into the twin-screw extruder, mix, extrude, cool, crush, and sieve to obtain the wear-resistant polyester resin powder coating.

Citation Information

Patent Citations

  • Nanopowder coating with super abrasion resistance

    CN105733419A

  • Deicing powder coating and preparation method thereof

    CN110183929A

  • High-weather-resistance powder coating for metal guardrails as well as preparation method and application of high-weather-resistance powder coating

    CN114133844A

  • Impact-resistant coating for impact-resistant forming net as well as preparation method and coating method of impact-resistant coating

    CN116334925A