A thermal insulation hydrophobic coating for building exterior wall and preparation method thereof

Through the combined use of modified polyurethane resin and silica nanoparticles, the problem of traditional materials being difficult to balance thermal insulation and hydrophobic properties is solved, achieving excellent performance and safety of building exterior wall coatings, and avoiding the risk of spontaneous combustion at high temperatures. .

CN118064045BActive Publication Date: 2024-10-18SHANGHAI YUCHANG CONSTR ENG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410199442.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-23
Publication Date
2024-10-18
Estimated Expiration
2044-02-23

AI Technical Summary

Technical Problem

Traditional building exterior wall insulation and hydrophobic materials are difficult to achieve both high-efficiency thermal insulation and hydrophobic properties, and are prone to spontaneous combustion at high temperatures, producing highly toxic gases and posing safety risks.

Method used

Modified polyurethane resin and modified silica nanoparticles are used as the main materials, and the hydrophobic properties of the coating are enhanced through chemical modifications such as phenylalanine, cationic surfactants and silane coupling agents, and through silane coupling agents Combined with the surface of nano-silica, it improves the dispersion and thermal stability of the coating, forming a coating with excellent insulation and hydrophobic properties.

Benefits of technology

It achieves good thermal insulation and hydrophobic properties of the building exterior wall coating, improves the hardness and adhesion of the coating, reduces hydrophilicity, and enhances the safety and durability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a thermal insulation hydrophobic coating for a building exterior wall and a preparation method thereof, and belongs to the technical field of thermal insulation hydrophobic coatings. The thermal insulation hydrophobic coating for a building exterior wall is prepared by emulsion polymerization of a modified polyurethane resin, modified nano silicon dioxide, gypsum filler, deionized water and other additives to obtain a thermal insulation hydrophobic coating for a building exterior wall. The coating prepared by the present invention has good thermal insulation and hydrophobic properties, and broadens the development of polyurethane in the field of thermal insulation materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings and relates to a thermal insulation hydrophobic coating for an exterior wall of a building and a preparation method thereof. Background Art

[0002] Nowadays, the construction industry has become one of the largest energy-consuming industries in the world. In particular, the widespread use of various refrigeration equipment has caused a sharp increase in energy consumption in the construction industry. Therefore, the issue of building energy conservation has received widespread attention from the entire industry. Among them, reducing the heat dissipation of buildings and improving the indoor thermal insulation performance is one of the most effective ways to reduce building energy consumption.

[0003] Under the development trend of energy conservation and environmental protection, thermal insulation coatings have been widely used in construction, oil pipelines, military equipment and other fields due to their good thermal barrier ability, simple construction and easy maintenance. The development and application of building thermal insulation coatings is an effective way to solve the problem of building energy conservation.

[0004] At the same time, in order to increase the service life of the building's exterior walls, the improvement of the hydrophobicity of the building's exterior walls is also a point of particular concern, because excessive humidity will lead to reduced mechanical strength of building materials, destructive deformation, and decay of organic materials, thereby reducing the quality and durability of the building. Polyurethane materials are foamed by chemical reactions under the action of catalysts, foaming agents, surfactants, etc., and have the characteristics of light weight, low thermal conductivity, simple operation and good bonding effect. However, this substance is very easy to spontaneously combust at high temperatures and will produce highly toxic gases.

[0005] At the same time, traditional wall insulation and hydrophobic materials have the disadvantages of not being able to have both properties and having poor effects. In order to achieve a coating that has both high-efficiency thermal insulation performance and meets the hydrophobic requirements, new functional materials need to be developed to overcome these problems. Summary of the invention

[0006] The object of the present invention is to provide a thermal insulation and hydrophobic coating for the exterior wall of a building and a preparation method thereof, which has good thermal insulation and hydrophobic properties.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The thermal insulation hydrophobic coating comprises the following parts: 20-45% of modified polyurethane resin, 30-45% of filler, 10% of deionized water and 1-5% of other additives;

[0009] As a preferred technical solution of the present invention, the modified polyurethane resin is prepared as follows:

[0010] Add polyurethane resin to a mixed solution of anhydrous ethanol and deionized water, heat to 90°C in a stirrer until the resin is completely dissolved, add 1-2 wt% of phenylalanine and 0-1.5 wt% of epoxy silane coupling agent, and react in a stirrer for 5-6 hours to obtain solution A;

[0011] Add 1 to 3 wt% of a cationic surfactant to solution A and stir thoroughly for 2 to 3 h to obtain solution B;

[0012] Add a curing agent to solution B and stir evenly to obtain a modified polyurethane resin with a hydrophobic effect.

[0013] As a preferred technical solution of the present invention, the filler is modified silicon dioxide nanoparticles, and the specific preparation process is as follows:

[0014] Grind the gypsum solid in a ball mill at a speed of 1500 r / min until the solid is completely powdered, sieve it to a mesh size of 200-400 mesh, and dry it in an oven at 100°C.

[0015] Nano-silica with a particle size of 100 to 200 nm was dried at 100 °C for 3 h, added to a high-speed mixer, and n-octyltrimethoxysilane coupling agent diluted with anhydrous ethanol was added, and then lauric acid and polyvinyl alcohol were added to treat the surface. n-octyltrimethoxysilane was reacted with the hydroxyl group on the nano-silica and connected with the alkyl group of the silane coupling agent. After fully stirring for 3 to 4 h, gypsum powder was added, and the mixture was fully stirred and reacted at room temperature for 5 h to prepare modified silica nanoparticles by a sol-gel method.

[0016] As a preferred technical solution of the present invention, the preparation process of the thermal insulation hydrophobic coating is as follows:

[0017] In a stirrer, add 10% water and 0.1-0.5 wt% of a dispersant and 0.1-0.5 wt% of a wetting agent, the speed is 1200 r / min, and magnetic stirring is performed for 0.5-1 h to ensure that different additives are evenly mixed in the water; add 20-45 wt% of a modified polyurethane resin, stir for 30 min, add 30-45 wt% of modified silica nanoparticles, increase the speed and stir for 3 h, the speed is 2000 r / min; add 2-4 wt% of a film-forming aid and 0-1 wt% of a defoamer and stir for half an hour, add 0.5-1 wt% of a thickener, add 0.5-1 wt% of a rust inhibitor, stir fully until the bubbles are eliminated, and then obtain a thermal insulation hydrophobic coating;

[0018] The thermal insulation hydrophobic coating is applied on the exterior wall of the building and naturally cured at room temperature for 12-24 hours to obtain the thermal insulation hydrophobic coating for the exterior wall of the building.

[0019] As a preferred technical solution of the present invention, the other additives include thickeners, dispersants, wetting agents, defoamers, film-forming aids, and rust inhibitors.

[0020] As a preferred technical solution of the present invention, the molar coefficient ratio of phenylalanine, epoxy silane coupling agent, polyurethane resin and curing agent is 0.5:1:10:1.

[0021] As a preferred technical solution of the present invention, the cationic surfactant is potassium monododecyl phosphate or hexadecyl dimethyl ammonium chloride.

[0022] As a preferred technical solution of the present invention, the mass ratio of the nano-silicon dioxide to gypsum is 10:1-3.

[0023] As a preferred technical solution of the present invention, the mass ratio of lauric acid, polyvinyl alcohol, n-octyltrimethoxysilane and nano-silicon dioxide is 1:1:1:30.

[0024] Beneficial effects of the present invention:

[0025] (1) Using polyurethane resin as the matrix, taking advantage of the good thermal insulation properties of polyurethane itself, the polyurethane is modified by the hydrophobic agent phenylalanine. After hydrolysis, the polyurethane main chain is connected to the small molecule of the hydrophobic agent through a silane coupling agent. Phenylalanine is connected to the main chain through the coupling agent, and the hydrophobic effect of the benzene ring is increased by the orderly arrangement on the polyurethane surface. The carboxyl group of phenylalanine participates in the reaction, removes the hydroxyl group, and the system is negatively charged. Further, the cationic surfactant potassium monododecyl phosphate is added, and the polar group of the cationic surfactant is close to the polyurethane main chain. The long-chain alkyl group of the hydrophobic effect faces the water phase, which further enhances the hydrophobic effect of the polymer surface. The hydrophobic ability is improved through the synergistic effect of phenylalanine and potassium monododecyl phosphate.

[0026] (2) Silica is a good coating filler with excellent thermal insulation properties. It is modified by adding the hydrophobic agent lauric acid and adding a coupling agent to increase the dispersibility of the filler, which can improve the mechanical properties and thermal stability of the polyurethane resin coating. At the same time, lauric acid is combined with the surface of nano-silica through the silane coupling agent. The silane coupling agent is connected to the hydroxyl group on the surface of silica through hydrolysis, thereby improving the hydrophobicity of the surface of nano-silica. Gypsum, as a sulfide mineral, has good thermal insulation properties. It is fully dispersed by the silane coupling agent and mixed with nano-silica to form a composite filler to form a good hydrophobic filler. When mixed with polyurethane to prepare a coating, it can reduce the hydrophilicity of the polyurethane coating and improve the hardness and adhesion of the coating, thereby obtaining a coating with excellent thermal insulation and hydrophobic properties. DETAILED DESCRIPTION

[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0028] Example 1

[0029] Preparation of modified polyurethane resin:

[0030] Add 20 wt% of polyurethane resin to a mixed solution of anhydrous ethanol and deionized water, heat to 90°C in a stirrer until the resin is completely dissolved, add 1 wt% of phenylalanine and 2 wt% of epoxy silane coupling agent, and react in a stirrer for 5 to 6 hours to obtain solution A;

[0031] Add 2 wt% of cationic surfactant potassium monododecyl phosphate to solution A and stir thoroughly for 2 to 3 hours to obtain solution B;

[0032] 2 wt % of a curing agent was added to solution B and stirred evenly to obtain a modified polyurethane resin having a hydrophobic effect.

[0033] The modified silica nanoparticles were prepared as follows:

[0034] Grind the gypsum solid in a ball mill at a speed of 1500 r / min until the solid is completely powdered, sieve it to a mesh size of 200-400 mesh, and dry it in an oven at 100°C.

[0035] Nano-silica with a particle size of 200 nm was dried at 100 °C for 3 h, added to a high-speed mixer, and a silane coupling agent of n-octyltrimethoxysilane diluted with anhydrous ethanol was added, and then 1 wt% of lauric acid and 1 wt% of polyvinyl alcohol were added to treat the surface. 1 wt% of n-octyltrimethoxysilane was used to react with the hydroxyl groups on the nano-silica and grafted with the alkyl chain of the silane coupling agent to form a hybrid network. After fully stirring for 3 to 4 h, 10 wt% of gypsum powder and 20 wt% of nano-silica were added, and the mixture was fully stirred and reacted at room temperature for 5 h to prepare modified silica nanoparticles by a sol-gel method.

[0036] The preparation process of the thermal insulation hydrophobic coating is as follows:

[0037] In a stirrer, add 10% water, 0.5 wt% dispersant and 0.5 wt% wetting agent, the speed is 1200r / min, and magnetic stirring is performed for 1 hour to ensure that different additives are evenly mixed in water; add 45 wt% modified polyurethane resin, stir for 30 minutes, add 40 wt% modified silica nanoparticles, increase the speed and stir for 3 hours, the speed is 2000 r / min; add 2 wt% film-forming aid and 1 wt% defoamer and stir for half an hour, add 0.5 wt% thickener, add 0.5wt% rust inhibitor, and wait until the bubbles are eliminated to obtain a thermal insulation hydrophobic coating;

[0038] The thermal insulation hydrophobic coating is applied on the exterior wall of the building and naturally cured at room temperature for 12-24 hours to obtain the thermal insulation hydrophobic coating for the exterior wall of the building.

[0039] Example 2

[0040] Preparation of modified polyurethane resin:

[0041] Add 20 wt% of polyurethane resin to a mixed solution of anhydrous ethanol and deionized water, heat to 90°C in a stirrer until the resin is completely dissolved, then add 1.5 wt% of phenylalanine and 1 wt% of epoxy silane coupling agent, and react in a stirrer for 5 to 6 hours to obtain solution A;

[0042] Add 1.5 wt% of cationic surfactant potassium monododecyl phosphate to solution A and stir thoroughly for 2-3 hours to obtain solution B;

[0043] 2 wt % of a curing agent was added to solution B and stirred evenly to obtain a modified polyurethane resin having a hydrophobic effect.

[0044] The modified silica nanoparticles were prepared as follows:

[0045] Grind the gypsum solid in a ball mill at a speed of 1500 r / min until the solid is completely powdered, sieve it to a mesh size of 200-400 mesh, and dry it in an oven at 100°C.

[0046] Nano-silica with a particle size of 200 nm was dried at 100 °C for 3 h and then added to a high-speed mixer. The surface was treated with n-octyltrimethoxysilane coupling agent diluted with anhydrous ethanol, 1 wt% lauric acid, and 1 wt% polyvinyl alcohol. 1 wt% n-octyltrimethoxysilane was used to react with the hydroxyl groups on the nano-silica and grafted with the alkyl chain of the silane coupling agent to form a hybrid network. After fully stirring for 3 to 4 h, 15 wt% gypsum powder and 15 wt% nano-silica were added. The mixture was fully stirred and reacted at room temperature for 5 h to prepare modified silica nanoparticles by a sol-gel method.

[0047] The process of preparing the thermal insulation hydrophobic coating is as follows:

[0048] In a stirrer, add 10% water, 0.5 wt% dispersant and 0.5 wt% wetting agent, the speed is 1200r / min, and magnetic stirring is performed for 1 h to ensure that different additives are evenly mixed in water; add 45 wt% modified polyurethane resin, stir for 30 min, add 40wt% modified silica nanoparticles, increase the speed and stir for 3 h, the speed is 2000 r / min; add 2 wt% film-forming aid and 1 wt% defoamer and stir for half an hour, add 0.5 wt% thickener, add 0.5wt% thickener, stir well, and obtain a thermal insulation hydrophobic coating when bubbles are eliminated;

[0049] The thermal insulation hydrophobic coating is applied on the exterior wall of the building and naturally cured at room temperature for 18 h to obtain the thermal insulation hydrophobic coating for the exterior wall of the building.

[0050] Example 3

[0051] Preparation of modified polyurethane resin:

[0052] 20 wt% of polyurethane resin was added to a mixed solution of anhydrous ethanol and deionized water, and the mixture was heated to 90°C in a stirrer until the resin was completely dissolved. 2 wt% of phenylalanine and 1 wt% of epoxy silane coupling agent were added, and the mixture was reacted in a stirrer for 6 h to obtain solution A.

[0053] 1.5 wt% of cationic surfactant potassium monododecyl phosphate was added to solution A and stirred for 3 h to obtain solution B;

[0054] 2 wt % of a curing agent was added to solution B and stirred evenly to obtain a modified polyurethane resin having a hydrophobic effect.

[0055] Preparation of modified silica nanoparticles:

[0056] Grind the gypsum solid in a ball mill at a speed of 1500 r / min until the solid is completely powdered, sieve it to a mesh size of 200-400 mesh, and dry it in an oven at 100°C.

[0057] Nano-silica with a particle size of 200 nm was dried at 100 °C for 3 h, added to a high-speed mixer, and n-octyltrimethoxysilane coupling agent diluted with anhydrous ethanol was added, 1 wt% of lauric acid and 1 wt% of polyvinyl alcohol were added to treat the surface, 1 wt% of n-octyltrimethoxysilane was used to react with the hydroxyl groups on the nano-silica and grafted with the alkyl chain of the silane coupling agent to form a hybrid network, after fully stirring for 3 to 4 h, 15 wt% of gypsum powder and 30 wt% of nano-silica were added, and the mixture was fully stirred and reacted at room temperature for 5 h to prepare modified silica nanoparticles by a sol-gel method.

[0058] Preparation of thermal insulation hydrophobic coating:

[0059] In a stirrer, add 10% water, 0.5 wt% dispersant and 0.5 wt% wetting agent, the speed is 1200r / min, and magnetic stirring is performed for 0.5-1 h to ensure that different additives are evenly mixed in water; add 45 wt% modified polyurethane resin, stir for 30 min, add 40 wt% modified silica nanoparticles, increase the speed and stir for 3 h, the speed is 2000r / min; add 2 wt% film-forming aid and 1 wt% defoamer and stir for half an hour, add 1 wt% thickener, and wait until the bubbles are eliminated to obtain a thermal insulation hydrophobic coating;

[0060] The thermal insulation hydrophobic coating is applied on the exterior wall of the building and naturally cured at room temperature for 18 h to obtain the thermal insulation hydrophobic coating for the exterior wall of the building.

[0061] Comparative Example 1

[0062] The difference between Comparative Example 1 and Example 1 is that potassium monododecyl phosphate is not added when preparing the modified polyurethane resin, and the other operations are the same.

[0063] Preparation of modified polyurethane resin:

[0064] 20 wt% of polyurethane resin was added to a mixed solution of anhydrous ethanol and deionized water, and the mixture was heated to 90 °C in a stirrer until the resin was completely dissolved. 1 wt% of phenylalanine and 2 wt% of epoxy silane coupling agent were added, and the mixture was reacted in a stirrer for 6 h. 2 wt% of a curing agent was added, and the mixture was stirred evenly to obtain a modified polyurethane resin with a hydrophobic effect.

[0065] Comparative Example 2

[0066] The difference between Comparative Example 2 and Example 1 is that phenylalanine is not added when preparing the modified polyurethane resin, and the other operations are the same.

[0067] Preparation of modified polyurethane resin:

[0068] 20 wt% of polyurethane resin and 2 wt% of cationic surfactant potassium monododecyl phosphate were added to a mixed solution of anhydrous ethanol and deionized water, and the mixture was stirred for 3 h. 2 wt% of curing agent was added and stirred evenly to obtain a modified polyurethane resin with hydrophobic effect.

[0069] Comparative Example 3

[0070] The difference between Comparative Example 3 and Example 1 is that lauric acid is not added when preparing the modified filler, and the other operations are the same.

[0071] Comparative Example 4

[0072] The difference between Comparative Example 4 and Example 1 is that no gypsum is added when preparing the modified filler, and the other operations are the same.

[0073] The coatings obtained in the above Examples 1-3 and Comparative Examples 1-4 were subjected to performance tests. The test methods are as follows. The results are shown in Table 1.

[0074] The thermal conductivity coefficient is determined in accordance with the provisions of the national standard GB / T25261-2018.

[0075] Table 1

[0076]

[0077] It can be seen from the above test data that the present invention discloses a thermal insulation hydrophobic coating for the exterior wall of a building and a preparation method thereof. The process design is reasonable, and the prepared polyurethane coating not only has excellent thermal insulation performance, but also excellent hydrophobic performance, and can be widely used in building surface coating.

[0078] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A thermal insulation hydrophobic coating for building exterior walls, Features: The thermal insulation hydrophobic coating comprises the following parts: 20-45% of modified polyurethane resin, 30-45% of filler, 10% of deionized water and 1-5% of other additives; wherein the other additives include thickeners, dispersants, wetting agents, defoamers, film-forming aids, and rust inhibitors; The preparation process of the modified polyurethane resin is as follows: S1. Add polyurethane resin to a mixed solution of anhydrous ethanol and deionized water, heat to 90°C in a stirrer until the resin is completely dissolved, add 1-2 wt% of phenylalanine and 0-1.5 wt% of epoxy silane coupling agent, and react in a stirrer for 5-6 h to obtain solution A; S2. Add 1 to 3 wt% of a cationic surfactant to solution A and stir thoroughly for 2 to 3 h to obtain solution B; S3, adding a curing agent to solution B, stirring evenly to obtain a modified polyurethane resin with a hydrophobic effect, wherein the mass ratio of the phenylalanine, epoxy silane coupling agent, polyurethane resin, and curing agent is 0.5:1:10:1; The filler described herein is modified silicon dioxide nanoparticles, and the specific preparation process is as follows: Grind the gypsum solid in a ball mill at a speed of 1500 r / min until the solid is completely powdered, sieve it to a mesh size of 200-400 mesh, and dry it in an oven at 100°C. Nano-silica with a particle size of 100 to 200 nm is dried at 100 °C for 3 h, added to a high-speed mixer, and n-octyltrimethoxysilane coupling agent diluted with anhydrous ethanol is added, and then lauric acid and polyvinyl alcohol are added to treat the surface, and n-octyltrimethoxysilane is reacted with hydroxyl groups on the nano-silica and connected with the silane coupling agent, and stirred for 3 to 4 h, and then gypsum powder is added, stirred and reacted at room temperature for 5 h, and modified silica nanoparticles are prepared by a sol-gel method, wherein the mass ratio of the nano-silica to the gypsum is 10:1-3, and the mass ratio of the lauric acid, polyvinyl alcohol, n-octyltrimethoxysilane to the nano-silica is 1:1:1:

30.

2. The building exterior wall thermal insulation hydrophobic coating according to claim 1, Features: The cationic surfactant is potassium monododecyl phosphate or hexadecyl dimethyl ammonium chloride.

3. A method for preparing a building exterior wall thermal insulation hydrophobic coating as claimed in any one of claims 1 to 2, Features: The preparation process of the thermal insulation hydrophobic coating is as follows: S31. In a stirrer, add 10% deionized water, 0.1-0.5 wt% dispersant and 0.1-0.5 wt% wetting agent, the speed is 1200 r / min, and magnetic stirring is performed for 0.5-1 h to ensure that different additives are evenly mixed in water; add 20-45 wt% modified polyurethane resin, stir for 30 min, add 30-45 wt% modified silica nanoparticles, increase the speed and stir for 3 h, the speed is 2000 r / min, add 2-4 wt% film-forming aid and 0-1 wt% defoamer and stir for half an hour, add 0.5-1 wt% thickener and 0.5-1 wt% rust inhibitor, stir thoroughly until bubbles are eliminated to obtain a thermal insulation hydrophobic coating; S32, applying the thermal insulation hydrophobic coating on the exterior wall of the building, and naturally curing it at room temperature for 12 to 24 hours to obtain the thermal insulation hydrophobic coating on the exterior wall of the building.

Citation Information

Patent Citations

  • Method for preparing lyophobic heat conduction material with micro-nano core-shell structure

    CN103146197A

  • Super-hydrophobic anticorrosive coating used for power transmission and transformation devices, and preparation method thereof

    CN106519955A

  • Single-component self-crosslinking waterborne polyurethane flame-retardant dispersion liquid as well as preparation method and application thereof

    CN109206585A

  • Thermal insulation coating for building exterior walls and preparation method of thermal insulation coating

    CN110484119A