A metakaolin-based refractory castable binder and its preparation method and application
By using the Al2O3-SiO2-BaO ternary system formed by metakaolin, barium hydroxide and barium aluminate, the problem of low melting point phase generation and high energy consumption in refractory castables is solved, achieving low energy consumption, low carbon, and high temperature performance. Development of refractory castable materials.
Patent Information
- Application Number
- CN202410236423.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-01
AI Technical Summary
Calcium aluminate cement used as a binding agent in existing refractory castables has the problems of low melting point phase formation and high production energy consumption. Traditional geopolymers are limited in use in high temperature environments.
Using metakaolin as raw material, barium hydroxide as alkaline activator, and barium aluminate as coagulant, a ternary system of Al2O3-SiO2-BaO is formed to generate barium feldspar, which has a high melting point and low thermal expansion coefficient, combined with silicon oxide Or aluminum oxide as an additive to improve hardening strength and reduce costs.
The development of low-energy, low-carbon, calcium-free cementitious materials has been achieved. It has good high-temperature performance, low thermal expansion, thermal insulation effect and high interface bonding strength, and is suitable for high-temperature industrial fields.
Smart Images

Figure CN118084511B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of refractory materials, and more specifically to a metakaolin-based refractory castable binder and a preparation method and application thereof. Background Art
[0002] Refractory materials are essential basic materials for high-temperature industries. Among them, refractory castables have the advantages of simple production process, low energy consumption, convenient construction and strong applicability, and are widely used in high-temperature industries such as metallurgy, glass and cement. The development and application of low-energy consumption and high-performance castables is an inevitable trend in the development of related fields under the background of the "dual carbon" strategy.
[0003] The binder in refractory castables can bind aggregates and fine powders so that they can obtain sufficient demoulding strength after curing. The binder not only determines the construction performance of the castable, but also has a significant impact on its high-temperature service behavior. Calcium aluminate cement has a suitable setting and hardening speed, high early strength, excellent high temperature resistance and wear resistance, and is a commonly used binder in castables. However, there are two prominent problems when using calcium aluminate cement as a castable binder: on the one hand, the CaO introduced in calcium aluminate cement can react with SiO2 to form low-melting-point phases such as calcium plagioclase (CaAl2Si2O8) and calcium aluminum feldspar (Ca2Al2SiO7), which affects the high-temperature performance of the castable; on the other hand, calcium aluminate cement is usually produced using alumina and limestone as raw materials using the traditional sintering method, which has a long process, complex technology, and high energy consumption.
[0004] Geopolymers can be made from aluminum-silicon raw materials with volcanic ash activity. They have strong binding ability, abundant raw materials, and low energy consumption in the production process. However, since traditional geopolymers use potassium hydroxide, sodium hydroxide, etc. as activators, they cannot be used in the field of high-temperature materials. Therefore, in order to develop low-carbon calcium-free gelling binders for refractory castables, it is necessary to study alkaline activators and hardening accelerators for high temperature use. Summary of the invention
[0005] In order to overcome the above technical problems, the present invention provides a metakaolin-based refractory castable binder and a preparation method and application thereof. The present invention uses metakaolin as a raw material, barium hydroxide as an alkaline activator, and then uses barium aluminate as a coagulant to prepare a metakaolin-based refractory castable binder. In a high temperature environment, the Al2O3-SiO2-BaO ternary system can react to generate celsium feldspar, which has a high melting point, a low thermal expansion coefficient, and good high-temperature performance, and is conducive to use in the field of high-temperature materials.
[0006] The first object of the present invention is to provide a metakaolin-based refractory castable binder, including a reaction main material, which includes the following components in mass percentage: 5-30% barium aluminate, 5-30% barium hydroxide, and the rest is metakaolin, totaling 100%.
[0007] In a preferred embodiment of the present invention, the main reaction material further includes an additive A, and the additive A is one or both of silicon oxide and aluminum oxide.
[0008] In a preferred embodiment of the present invention, the ratio of the total mass of metakaolin, barium monoaluminate and barium hydroxide to the mass of additive A is 1-4:1.
[0009] In a preferred embodiment of the present invention, an additive B is also included, and the additive B is sodium tripolyphosphate.
[0010] In a preferred embodiment of the present invention, the amount of additive B added is 1% of the mass of the main reaction material.
[0011] In a preferred embodiment of the present invention, the metakaolin is obtained by calcining kaolin at 600-900°C.
[0012] In a preferred embodiment of the present invention, barium aluminate is obtained by mixing BaCO3 and Al(OH)3 and calcining the mixture at 1200-1400°C.
[0013] In a preferred embodiment of the present invention, the molar ratio of BaCO3 to Al(OH)3 is 1:2.
[0014] The second object of the present invention is to provide a method for preparing the above-mentioned metakaolin-based refractory castable binder, wherein the metakaolin-based refractory castable binder is obtained by weighing the main reaction material according to the formula or mixing the main reaction material with the additive B uniformly.
[0015] The second object of the present invention is to use the above-mentioned metakaolin-based refractory castable binder in the preparation of refractory materials.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The present invention uses metakaolin as a raw material, barium hydroxide as an alkaline activator, and then barium aluminate as a coagulant. The metakaolin has volcanic ash activity and contains a large amount of amorphous Al2O3 and SiO2. The silicon-aluminum oxide compound undergoes a process from depolymerization to repolymerization to prepare a binder for a metakaolin-based refractory castable. Under a high temperature environment, the Al2O3-SiO2-BaO ternary system can react to generate barium feldspar, which has a high melting point (1760°C), a low thermal expansion coefficient, and good high temperature performance.
[0018] The present invention has the following advantages in the preparation process: (a) The energy consumption and CO2 emissions of the production process are lower than those of cement, the calcination temperature for preparing geopolymer raw materials is relatively low (600-900°C), and carbonates such as limestone are not used in the production process. (b) The construction performance is good, the preparation process is simple, and it can harden quickly at room temperature. (c) The thermal insulation effect is good, and the thermal conductivity is as low as 0.24-0.38W / (m·K). (d) The interface bonding strength is high, and there is no large crystal transition area at the bonding interface in the material. (e) The hydration heat is low, and it will not cause a sharp temperature rise during the curing process, thereby avoiding the damage caused by thermal stress.
[0019] (2) Replacing alumina or silica powder with metakaolin can save costs, and mullite formed at high temperatures can reduce the thermal expansion coefficient of the castable. Using barium hydroxide as an alkaline activator can ensure the high-temperature performance of the castable, and introducing barium aluminate can improve the hardening strength of the castable. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The XRD patterns of the binders prepared in Example 8 and Comparative Example 1 after being treated at different temperatures of 1100°C (a) and 1550°C (b);
[0021] Figure 2 The room temperature elastic modulus (a), room temperature flexural strength (b) and room temperature compressive strength (c) of the castable after being treated at different temperatures. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Traditional geopolymers use potassium hydroxide, sodium hydroxide, etc. as activators, which makes them incapable of being used in the field of high-temperature materials. Although Ba(OH)2 has strong alkalinity and barium aluminate has high hydration activity, there are no reports of cementitious materials using Ba(OH)2 as an alkaline activator and barium aluminate as a coagulant. Based on this, the present invention proposes to prepare cementitious materials using metakaolin as aluminosilicate raw material, Ba(OH)2 as an alkaline activator, and barium aluminate as a coagulant, which is of great significance for the development of low-carbon calcium-free cementitious materials for high-temperature use.
[0024] The invention provides a metakaolin-based refractory castable binder, which comprises a reaction main material, wherein the reaction main material comprises the following components in mass percentage: 5-30% of barium aluminate, 5-30% of barium hydroxide, and the rest of metakaolin, which is 100% in total.
[0025] Barium aluminate (BaAl2O4) in the Al2O3-BaO binary system has high thermal stability and its hydraulic properties are similar to those of calcium aluminate cement. It is the main mineral of barium cement. At the same time, it has high refractoriness (above 1850℃), good thermal shock resistance, short setting and hardening time, and can react with Al2O3 at high temperatures to form barium hexaaluminate (BaAl 12 O 19 ). The solubility of barium ions in alkali is higher, and the alkalinity is stronger than that of sodium hydroxide. In addition, at high temperatures, the Al2O3-SiO2-BaO ternary system can react to form barium feldspar (BaAl2Si2O8), which has a high melting point (1760°C), a low thermal expansion coefficient, and good high-temperature performance.
[0026] Under alkaline conditions, metakaolin can undergo depolymerization-polymerization reaction to form geopolymers containing silicon-oxygen tetrahedrons and aluminum-oxygen tetrahedrons. Barium aluminate can undergo hydration reaction when it meets water to form a series of hydration products such as hydrated barium aluminate. In the presence of active aluminosilicate minerals, hydration products such as hydrated barium aluminosilicate can also be formed.
[0027] In one embodiment of the present invention, the main reaction material further includes additive A, and additive A is one or both of silicon oxide and aluminum oxide. Additive A can play a role in composite gelation, and can be used in combination with metakaolin, which can further improve the initial hardening strength of metakaolin-bonded refractory castables and shorten the setting time. Specifically, the added additive A can participate in the gelation reaction of the above three raw materials to form the binder as an aluminum-silicon active raw material, and can also undergo hydration or coagulation reaction alone.
[0028] In one embodiment of the present invention, the ratio of the total mass of metakaolin, barium monoaluminate and barium hydroxide to the mass of additive A is 1-4:1.
[0029] The mass ratio of the total mass of metakaolin, barium monoaluminate and barium hydroxide to the additive A can be adjusted according to the chemical composition or performance requirements of the castable.
[0030] In one embodiment of the present invention, an additive B is also included, and the additive B is sodium tripolyphosphate. The additive B is used to disperse the raw materials and reduce the amount of water added to the castable.
[0031] In one embodiment of the present invention, the amount of additive B added is 0.5%-2% of the mass of the main reaction material.
[0032] During the preparation process, the type and proportion of material powders are changed to adjust the amount of additive B, thereby changing the amount of water added and the fluidity of the castable.
[0033] In one embodiment of the present invention, the metakaolin is obtained by calcining kaolin at 600-900° C. Aluminosilicate minerals such as kaolin can be calcined at a certain temperature to generate metakaolin in a metastable state.
[0034] In one embodiment of the present invention, barium aluminate is obtained by mixing BaCO3 and Al(OH)3 and calcining at 1200-1400° C. Changing the calcination temperature will affect the purity and activity of the synthesized barium aluminate.
[0035] Further preferably, the molar ratio of BaCO3 to Al(OH)3 is 1:2.
[0036] The present invention also provides a method for preparing a metakaolin-based binder, and the specific technical scheme is as follows:
[0037] The main reaction material is weighed according to the formula, or the main reaction material and additive B are mixed evenly to obtain a metakaolin-based binder.
[0038] The metakaolin-based binder prepared by the present invention can be used for preparing refractory castables.
[0039] Example 1
[0040] This embodiment provides a metakaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 90% metakaolin, 5% barium aluminate, and 5% barium hydroxide.
[0041] The metakaolin used in this example was prepared by calcining kaolin at 750° C. for 3 hours.
[0042] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh when used.
[0043] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0044] According to the above formula, 600 g of the main reaction material was weighed, placed in a ball mill and blended at a speed of 300 rad / min for 2 h.
[0045] Example 2
[0046] This embodiment provides a metakaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by weight: 90% metakaolin, 5% barium aluminate, 5% barium hydroxide, and 1% sodium tripolyphosphate by weight of the main reaction material.
[0047] The metakaolin used in this example was prepared by calcining kaolin at 750°C for 3h;
[0048] The barium aluminate used in this embodiment is obtained by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0049] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0050] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage, and the mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0051] Example 3
[0052] This embodiment provides a metakaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 70% metakaolin, 15% barium aluminate, and 15% barium hydroxide.
[0053] The metakaolin used in this example is prepared by calcining kaolin at 750°C for 3 hours.
[0054] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0055] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0056] According to the above formula, 600 g of the main reaction material was weighed, placed in a ball mill and blended at a speed of 300 rad / min for 2 h.
[0057] Example 4
[0058] This embodiment provides a metakaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by weight: 70% metakaolin, 15% barium aluminate, 15% barium hydroxide, and 1% sodium tripolyphosphate by weight of the main reaction material.
[0059] The metakaolin used in this example is prepared by calcining kaolin at 750°C for 3 hours.
[0060] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0061] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0062] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage, and the mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0063] Example 5
[0064] This embodiment provides a metakaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 50% metakaolin, 25% barium aluminate, and 25% barium hydroxide.
[0065] The metakaolin used in this example is prepared by calcining kaolin at 750°C for 3 hours.
[0066] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0067] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0068] According to the above formula, 600 g of the main reaction material was weighed, placed in a ball mill and blended at a speed of 300 rad / min for 2 h.
[0069] Example 6
[0070] This embodiment provides a metakaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 50% metakaolin, 25% barium aluminate, 25% barium hydroxide, and 1% sodium tripolyphosphate by mass of the main reaction material.
[0071] The metakaolin used in this example is prepared by calcining kaolin at 750°C for 3 hours.
[0072] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0073] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0074] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage. The mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0075] Example 7
[0076] This embodiment provides a kaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 56% kaolin, 12% barium aluminate, 12% barium hydroxide, 20% silicon powder, and 1% sodium tripolyphosphate by mass of the main reaction material.
[0077] The metakaolin used in this example is prepared by calcining kaolin at 750°C for 3 hours.
[0078] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0079] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0080] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage. The mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0081] Example 8
[0082] This embodiment provides a kaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 52.5% kaolin, 11.25% barium aluminate, 11.25% barium hydroxide, 25% silicon powder, and 1% sodium tripolyphosphate by mass of the main reaction material.
[0083] The metakaolin used in this example is prepared by calcining kaolin at 750°C for 3 hours.
[0084] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1300°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0085] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0086] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage. The mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0087] Example 9
[0088] The present embodiment provides a kaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by weight: 46.2% kaolin, 10.4% barium aluminate, 10.4% barium hydroxide, 25% silicon powder, and 1% sodium tripolyphosphate by weight of the main reaction material.
[0089] The metakaolin used in this example was prepared by calcining kaolin at 600°C for 3 hours.
[0090] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1200°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0091] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0092] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage. The mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0093] Example 10
[0094] This embodiment provides a kaolin-based refractory castable binder, wherein the main reaction material is composed of the following components in percentage by mass: 35% kaolin, 7.5% barium aluminate, 7.5% barium hydroxide, 50% silicon micropowder, and 1% sodium tripolyphosphate by mass of the main reaction material.
[0095] The metakaolin used in this example was prepared by calcining kaolin at 900°C for 3 hours.
[0096] The barium aluminate used in this embodiment is synthesized by mixing BaCO3 and Al(OH)3 reagents and calcining them at 1400°C for 3 hours. The raw materials are crushed to less than 200 mesh.
[0097] In this embodiment, when preparing the metakaolin-based refractory castable binder, the preparation steps are as follows:
[0098] According to the above formula, 600 g of the main reaction material was weighed, and sodium tripolyphosphate was added according to the mass percentage. The mixture was placed in a ball mill and blended at a speed of 300 rad / min for 2 hours.
[0099] Comparative Example 1
[0100] This comparative example provides a refractory castable binder, wherein the main reaction material is composed of the following components in percentage by weight: 52.5% metakaolin, 11.25% Secar 71 cement (Secar71), 11.25% calcium hydroxide, 25% silica powder, and 1% sodium tripolyphosphate by weight of the main reaction material.
[0101] The metakaolin used in this comparative example was prepared by calcining kaolin at 750° C. for 3 hours.
[0102] In this comparative example, when preparing a metakaolin-based refractory castable binder, the preparation steps are as follows:
[0103] According to the above formula, 600 g of the main reaction material was weighed, placed in a ball mill and blended at a speed of 300 rad / min for 2 h.
[0104] The kaolin-based refractory castable binders prepared by Examples 1 to 10 can all generate barium feldspar and have good high-temperature performance. In order to further prove that the kaolin-based refractory castable binder prepared by the present invention can be used in a high-temperature environment, the following performance characterization tests are carried out at 1100°C (medium temperature) and 1550°C (high temperature) respectively using Example 8 and Comparative Example 1.
[0105] The metakaolin-based refractory castable binders prepared in Comparative Example 1 and Example 8 were mixed with corundum fine powder (325 mesh) in a ratio of 1:4, and then heat-treated at 1100°C and 1550°C for 3 hours. The prepared samples were marked as 1# and 2#, respectively. The phase compositions thereof were determined. The results are as follows: Figure 1 It can be seen that after treatment at 1100°C, calcium plagioclase (CaAl2Si2O8) appeared in sample 1#, while barium feldspar (BaAl2Si2O8) appeared in sample 2#. Similarly, when the heat treatment temperature was increased to 1550°C, sample 2# still contained BaAl2Si2O8, while calcium plagioclase (CaAl2Si2O8) did not appear in sample 1#. It may be that it reacted with other impurities to form a glass phase. It can be seen that the low-melting-point phase of CaAl2Si2O8 generated by the reaction of CaO with SiO2 will affect the high-temperature performance of the castable. In the present invention, barium feldspar (BaAl2Si2O8) can be reacted in the Al2O3-SiO2-BaO ternary system under high temperature conditions, which has a high melting point (1760°C), a low thermal expansion coefficient, and good high-temperature performance.
[0106] In order to further verify the high temperature performance of the metakaolin-based refractory castable binder prepared by the present invention, the present invention mixes the binder with other raw materials to prepare a castable, and the formula is shown in Table 1.
[0107] Table 1 Casting material formula (wt%)
[0108]
[0109] The No. 1 castable sample is composed of the following components in percentage by mass: 15wt% of 5-3mm corundum, 27wt% of 3-1mm corundum, 22wt% of 1-0mm corundum, 23wt% of 325 mesh corundum, 5wt% of activated alumina powder, and 7wt% of Secar71-silica powder-metakaolin;
[0110] The addition amount of sodium tripolyphosphate is 1wt% of the total mass of the above raw materials.
[0111] Secar71-silica powder-metakaolin refers to weighing 52.5% metakaolin, 11.25% Secar 71 cement (Secar71), 11.25% calcium hydroxide, and 25% silica powder according to the formula of Comparative Example 1.
[0112] The No. 1 castable sample was prepared according to the following steps:
[0113] Step (1), weigh 5-3 mm corundum, 3-1 mm corundum, 1-0 mm corundum, 325 mesh corundum, activated alumina powder and Secar71-silicon powder-metakaolin according to the above mass percentage, place 325 mesh corundum, activated alumina powder and Secar71-silicon powder-metakaolin in a ball mill and blend at a speed of 300 rad / min for 2 hours.
[0114] Step (2), weighing about 5% by mass of deionized water, dissolving 1% by mass of sodium tripolyphosphate in the water to prepare a solution; placing the weighed corundum aggregate and the ball-milled raw materials in a stirring pot and stirring for 3 minutes, adding the prepared sodium tripolyphosphate solution during the stirring process to obtain a mixed castable.
[0115] Step (3), pour the mixed casting material into a mold of 40mm×40mm×160mm, and vibrate it on a vibration table for 2 minutes. Then, place it in a constant temperature and humidity chamber (humidity 90%, temperature 25°C) for 24 hours and then demould it. After demoulding, place the sample in an oven at 110°C for 24 hours, take it out and cool it naturally to room temperature. The obtained sample is recorded as drying only.
[0116] In addition, the dried samples were heat treated at 1100°C and 1550°C, respectively, with a holding time of 3 h, to obtain test samples, which were recorded as 1100°C and 1550°C, respectively.
[0117] The No. 2 castable sample is composed of the following components in percentage by mass: 15wt% of 5-3mm corundum, 27wt% of 3-1mm corundum, 22wt% of 1-0mm corundum, 23wt% of 325 mesh corundum, 5wt% of activated alumina powder, and 7wt% of barium monoaluminate-silicon powder-metakaolin;
[0118] The addition amount of sodium tripolyphosphate is 1wt% of the total mass of the above raw materials.
[0119] Barium monoaluminate-silica powder-metakaolin refers to the formula of Example 8, which includes 52.5% metakaolin, 11.25% barium monoaluminate, 11.25% barium hydroxide, and 25% silica powder.
[0120] The No. 2 castable sample was prepared according to the following steps:
[0121] Step (1), according to the above mass percentage, weigh 5-3 mm corundum, 3-1 mm corundum, 1-0 mm corundum, 325 mesh corundum, activated alumina powder and barium aluminate-silicon powder-metakaolin, place the 325 mesh corundum, activated alumina powder and barium aluminate-silicon powder-metakaolin in a ball mill and blend them at a speed of 300 rad / min for 2 hours.
[0122] Step (2), weighing about 5% by mass of deionized water, dissolving 1% by mass of sodium tripolyphosphate in the water to prepare a solution; placing the weighed corundum aggregate and the ball-milled raw materials in a stirring pot and stirring for 3 minutes, adding the prepared sodium tripolyphosphate solution during the stirring process to obtain a mixed castable.
[0123] Step (3), pour the mixed casting material into a mold of 40mm*40mm*160mm, and vibrate it on a vibration table for 2 minutes. Then, place it in a constant temperature and humidity box (humidity 90%, temperature 25°C) for curing for 24 hours and then demould it. After demoulding, place the sample in an oven at 110°C for drying for 24 hours, take it out and cool it naturally to room temperature. The obtained sample is recorded as drying only.
[0124] In addition, the dried samples were heat treated at 1100°C and 1550°C, respectively, with a holding time of 3 h, to obtain test samples, which were recorded as 1100°C and 1550°C, respectively.
[0125] from Figure 2 It can be seen that the room temperature elastic modulus, room temperature flexural strength and room temperature compressive strength of castable No. 1 composed of Secar71-silica powder-metakaolin and castable No. 2 composed of barium aluminate-silica powder-metakaolin are similar, indicating that replacing calcium aluminate cement with barium aluminate has little effect on the room temperature strength of the castable.
[0126] The high temperature flexural strength of castable No. 1 and castable No. 2 which were dried only were tested at 1400°C, as shown in Table 2.
[0127] Table 2 High temperature flexural strength of castables with different compositions
[0128]
[0129] It can be seen from Table 2 that the high-temperature flexural strength of the castable prepared by the present invention using barium aluminate, silicon micropowder and kaolin as raw materials reaches 3.4 MPa, which is 89% higher than that of sample No. 1, indicating that the kaolin-based refractory castable binder prepared by the present invention has excellent high-temperature performance.
[0130] In the field of refractory materials, potassium and sodium are generally recognized as impurity elements that easily form low-melting-point phases, and their content should be eliminated or controlled as much as possible. Therefore, they cannot be used in the preparation of high-temperature materials. Based on this, the present invention uses kaolin as a raw material, barium hydroxide as an alkaline activator, and barium aluminate as a coagulant. Kaolin has volcanic ash activity and contains a large amount of amorphous Al2O3 and SiO2. Under the action of additives such as alkaline activators and coagulants, the silicon-aluminum oxide compound undergoes a process from depolymerization to repolymerization to form a geopolymer. Barium aluminate (BaAl2O4) in the Al2O3-BaO binary system has high thermal stability, and its hydraulic properties are similar to those of calcium aluminate cement. It is the main mineral of barium cement. At the same time, barium aluminate has high refractoriness (above 1850°C), good thermal shock stability, short coagulation and hardening time, and can also react with Al2O3 at high temperatures to form barium hexaaluminate (BaAl 12 O 19 ). The solubility of barium ions in alkali is higher, and the alkalinity is stronger than that of sodium hydroxide. In addition, under high temperature, the Al2O3-SiO2-BaO ternary system can react to form barium feldspar (BaAl2Si2O8), which has a high melting point (1760℃), a low thermal expansion coefficient, good high temperature performance, and can be used under high temperature conditions.
[0131] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0132] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A metakaolin-based refractory castable binder, characterized in that: It is composed of a main reaction material and an additive B; The main reaction materials are composed of barium aluminate, barium hydroxide, metakaolin and silicon powder; The mass percentage of barium aluminate in the main reaction material is 5-30%; The mass percentage of barium hydroxide in the main reaction material is 5-30%; The mass ratio of the total mass of metakaolin, barium aluminate and barium hydroxide to the mass of silica powder is 1:1, 3:1 or 4:1; Additive B is sodium tripolyphosphate; The amount of additive B added is 1% of the mass of the main reaction material.
2. A metakaolin-based refractory castable binder according to claim 1, characterized in that: Metakaolin is obtained by calcining kaolin at 600-900°C.
3. A metakaolin-based refractory castable binder according to claim 1, characterized in that: Barium aluminate is obtained by mixing BaCO3 and Al(OH)3 and calcining at 1200-1400°C.
4. A metakaolin-based refractory castable binder according to claim 3, characterized in that: The molar ratio of BaCO3 and Al(OH)3 is 1:
2.
5. A method for preparing the metakaolin-based refractory castable binder according to claim 1, characterized in that: The main reaction material and additive B are weighed according to the formula, and mixed evenly to obtain a metakaolin-based refractory castable binder.
6. Use of the metakaolin-based refractory castable binder according to claim 1 in the preparation of refractory materials.
Citation Information
Patent Citations
Alkali-activated binders, alkali-activated mortars using binders, concrete products, and wet red clay paving materials
CN102300826A
Geopolymer concrete composition
IN201811037203A