A powder injection molded silicon carbide copper composite material and preparation method thereof
By plating tungsten and copper metal layers on the surface of silicon carbide powder to form a composite layer modification process, the problems of poor wettability and sintering shrinkage of SiC/Cu composite materials are solved, and powder injection molding of SiC/Cu with high density and high thermal conductivity is achieved. Cu composite materials are suitable for a variety of electronic devices.
Patent Information
- Application Number
- CN202311745312.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-19
AI Technical Summary
It is difficult to effectively prepare SiC/Cu composite materials with high density and good thermal conductivity through the powder injection molding process with the existing technology. This is mainly due to the two-phase non-wetting and sintering shrinkage difficulties of the SiC/Cu composite material, which results in high processing difficulty and cost. high.
The surface of silicon carbide powder is covered with a composite coating, which is modified with tungsten and copper metal layers to form a tungsten/copper composite layer to improve the wettability of SiC/Cu composite materials. density of SiC/Cu composites.
It achieves high-density sintering of SiC/Cu composite materials, and the metallic copper is evenly distributed, which significantly improves the thermal conductivity and strength of the material. It is suitable for chip packaging, communication module heat dissipation and other fields.
Smart Images

Figure CN118106491B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of powder injection molding materials, and in particular to a powder injection molding silicon carbide copper composite material and a preparation method thereof. Background Art
[0002] Copper is one of the metals with the highest thermal conductivity and electrical conductivity. Pure copper and copper alloys are widely used due to their excellent electrical and thermal conductivity, as well as good corrosion resistance and fatigue performance. However, due to the low hardness and high thermal expansion coefficient of copper, the application of copper is limited to low expansion coefficient and high strength requirements. At present, the conventional practice is to use a two-phase composite method to retain the high thermal conductivity and high electrical conductivity of copper while obtaining high strength and low expansion coefficient, such as tungsten copper alloy, molybdenum copper alloy, silicon carbide copper composite material, etc. However, due to the high price and high density of metal materials such as tungsten and molybdenum, their use in certain occasions of composite with copper is limited. SiC has the advantages of high thermal conductivity, low expansion coefficient, high strength, high temperature resistance, and low price. It has good thermal conductivity, high strength and low expansion coefficient performance with copper composite materials and has received widespread attention.
[0003] Using tungsten carbide and copper or other metals to improve the comprehensive performance of composite materials has become one of the research hotspots in the field of metal materials. According to relevant research reports, SiC / Cu composite materials are a new type of structural material with good electrical conductivity, thermal conductivity, high strength, high temperature resistance, high wear resistance and low thermal expansion coefficient. They can be used in aerospace, electrodes, contacts, electronic packaging, optical communication modules and other fields. SiC / Cu composite materials have such excellent performance, but they also have some inherent disadvantages, mainly: (1) Silicon carbide is a carbide ceramic, while copper is a metal. The crystal structure and material properties of the two are very different, and the material wettability is poor. Generally, they can only be produced by hot pressing sintering, SPS discharge plasma sintering, pressure copper infiltration, electroforming, 3D printing and other processes. However, due to the limitations of the production process, they can only be made into simple shapes such as block and round cake-shaped structural blanks. The processing allowance is large, the subsequent processing cost is high and the processing is difficult, resulting in a very high total product cost, and even facing the problem of being unable to be processed; (2) Silicon carbide is very hard, with a Mohs hardness of up to 9.5, second only to diamond, making SiC / Cu composite materials very difficult to process, and even grinding processing technology cannot be selected.
[0004] For example, the invention patent CN201110047441 discloses a tungsten carbide / silicon carbide composite powder and its preparation method. The composite powder is made of silicon carbide particles as raw materials, and tungsten-containing reagents such as ammonium metatungstate, ammonium tungstate, sodium tungstate, etc. as tungsten sources. Tungsten oxide is coated on the surface of silicon carbide by acid precipitation, and tungsten oxide is then carburized to obtain tungsten carbide / silicon carbide composite powder. Tungsten carbide ceramics have good compatibility with metals such as nickel and cobalt. They are often used as tungsten carbide bonding phases in cemented carbides. On the premise of ensuring the wear resistance and high temperature resistance of the obtained materials, the application scope of SiC is broadened; tungsten carbide-coated silicon carbide composite powder can be used as a metal additive to enhance the wear resistance of the metal matrix, greatly reducing the wear cost of the metal matrix. However, this method obtains tungsten carbide-coated silicon carbide composite powder by chemical coating, and during the complex chemical reaction, the bonding strength of the coating is difficult to guarantee; in addition, the metals that have good wettability with tungsten carbide are only a few metals such as cobalt and nickel, and the application scope is limited.
[0005] For example, the invention patent CN201210429043 discloses a silicon carbide and copper-silicon alloy dual-continuous phase composite material and its preparation method, which is composed of 35-50vt% porous silicon carbide ceramics and 50-65vt% copper-silicon alloys. Its preparation method consists of two key process steps: sintering preparation of porous silicon carbide ceramic skeleton and vacuum infiltration of porous silicon carbide by copper-silicon alloy. Since silicon is used as an alloying element of copper, the wettability and reactivity problems between copper and silicon carbide are solved at the same time. This method belongs to the infiltration process, and belongs to different industries from the powder injection molding method of the present invention. Since the infiltration phase will be heated to above the melting point during the infiltration process, it will cause certain erosion to the skeleton agent, and only some simple shapes can be made, and the processing margin is also large. In addition, although the use of silicon-copper alloy for infiltration improves the surface wetting and reaction problems of copper and silicon carbide, the use of copper-silicon alloy instead of copper element will also lead to a significant decrease in the thermal conductivity of the material, and lose the advantages of SiC / Cu composite materials.
[0006] For example, the invention patent CN201310712881 discloses a nano-scale silicon carbide reinforced metal matrix composite material and its preparation method. The invention relates to a nano-scale silicon carbide reinforced metal matrix composite material and its preparation method. Nano-scale silicon carbide spherical powder and metal powder accounting for 0.1% to 25% by weight are uniformly mixed into a binder to obtain two premixes. The metal powder includes copper powder and others such as 316L stainless steel powder, 430L stainless steel powder, 304L stainless steel powder, 17 to 4pH stainless steel powder, 4J29 alloy powder, 4J32 alloy powder, etc. The two premixes are compounded in a mixer according to a certain ratio to form a uniform feed, and injection molding is performed accordingly, and the binder is removed and vacuum sintering is performed to obtain a composite material molded product. The invention uses β-phase silicon carbide nano-scale spherical powder as the reinforcing phase, and evenly mixes metal powder and β-phase silicon carbide nano-scale spherical powder into the corresponding binder, and combines rapid injection molding technology to achieve batch production. The relative density obtained thereby reaches 99%, which has the advantages of good performance and low cost. The main purpose of the invention is to strengthen metal with silicon carbide. Adding a small amount such as 1-2% by mass will improve the hardness and wear resistance of the composite material. However, since it is still a problem of interface wetting between silicon carbide and metal, the density will decrease rapidly after adding a high amount, and even the metal will precipitate to the surface of the blank and cannot be formed.
[0007] For example, invention patent CN202210540348 discloses a surface-modified silicon carbide particle-reinforced copper-based composite material and its preparation method. This method also uses a mechanical pressure infiltration process. In order to solve the problem of reaction between silicon carbide particles and copper matrix and insufficient wettability, a dual-temperature zone chemical vapor deposition furnace is used to plate zirconium metal on the surface of silicon carbide particles. It has excellent performance advantages for the surface modification requirements of industrial-scale silicon carbide particles. The prepared copper-based composite material has high density, low thermal expansion coefficient, and significantly improved thermal conductivity, which meets the urgent demand for high thermal conductivity thermal management materials for heat dissipation of high-power devices in the field of electronic packaging. This invention uses a mechanical pressure infiltration process. The silicon carbide zirconium-plated powder needs to undergo skeleton sintering and infiltration and high-temperature heating twice. It is inevitable that the zirconium metal will agglomerate and grow, and the zirconium coated on the surface of the silicon carbide powder will be lost or damaged. Zirconium and silicon carbide also have the problem of surface wetting. When the silicon carbide porous skeleton is sintered, the zirconium will separate due to the non-wetting of the two phases, and it will not play the role of wetting the copper metal surface during copper infiltration, resulting in certain problems in the densification and homogenization of the material.
[0008] Powder injection molding is a new component molding and processing technology formed by introducing plastic injection molding technology into the field of powder metallurgy. It is a near-net molding method that combines the high molding efficiency of plastic injection molding and the high performance of powder metallurgy molding of metals and ceramics. It is widely used in the processing of complex-shaped products such as metals and ceramics. It mixes powder (metal powder, ceramic powder or a combination of the two) with an organic binder into a uniform feed, granulates it, and then injects it into a molded blank, which is then degreased and sintered to become the desired finished product. Since this process is net-size molding, it has the advantages of high material utilization, can be directly molded into complex shapes, high batch production efficiency, and high dimensional accuracy, thereby achieving less or even no processing of the product.
[0009] Since the 1990s, powder injection molding technology has continued to develop rapidly, and more and more materials have been successfully commercially applied using injection molding technology. If the powder injection molding technology can be used for copper silicon carbide composite material processing, it can perfectly solve the shortcomings of copper silicon carbide material processing difficulty and difficulty in forming complex shapes. It can not only directly obtain high-precision near-molded products, reduce processing allowances, and avoid the shortcomings of silicon carbide difficult processing, but also the process is efficient and low-cost, suitable for mass production of products. However, the use of injection molding SiC / Cu composite material also has its difficulties, mainly because SiC / Cu composite material is a metal-based carbide ceramic composite material, the two materials have huge differences in properties, the two phases are not solid-dissolved, the interface is not wetted, sintering shrinkage is difficult, shrinkage during sintering is difficult to be dense, the melting point temperature is very different, and the sintering temperature is too high, copper will precipitate the material, and qualified sintering products cannot be obtained.
[0010] In summary, how to obtain SiC / Cu composite materials with high density and good thermal conductivity using powder injection molding technology is a technical problem that needs to be solved urgently. Summary of the invention
[0011] In view of this, the purpose of the present invention is to propose a powder injection molding silicon carbide copper composite material and a preparation method thereof, and to innovatively cover the surface of silicon carbide powder with a composite coating, thereby improving the non-wetting of the two phases and the reaction defects of the SiC / Cu composite material during sintering, and then to obtain a SiC / Cu composite material with high density and good thermal conductivity by a powder injection molding method.
[0012] Based on the above purpose, the present invention provides a powder injection molding silicon carbide copper composite material, comprising the following raw materials in mass percentage: 82-91.6% of inorganic mixed powder, 0-7.25% of paraffin wax, 0-2.5% of microcrystalline wax, 0-11.2% of polyoxymethylene, 0.5-5.4% of polyethylene, 0-0.6% of polypropylene, 0-1% of ethylene-vinyl acetate copolymer, 0-0.6% of polyamide, 0-0.6% of polyethylene glycol, 0-0.7% of polystyrene, 0-0.4% of dibutyl phthalate, and 0.3-0.7% of surfactant;
[0013] The inorganic mixed powder is composed of the following raw materials in mass percentage: 5-40% of modified SiC powder and the balance of Cu powder with laser particle size D50=5-11 μm;
[0014] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=1-7μm as a substrate, coating a tungsten film with a thickness of 0.5-1μm and a copper film with a thickness of 0.5-2μm on the surface of the substrate in sequence, and then maintaining the temperature at 550-600°C in a hydrogen atmosphere for 2-8h to obtain tungsten / copper modified SiC powder.
[0015] Furthermore, the surfactant is one of stearic acid or zinc stearate.
[0016] Furthermore, the powder injection molding silicon carbide copper composite material comprises the following raw materials in percentage by mass: 86.1% inorganic mixed powder, 0.2% paraffin wax, 11.2% polyoxymethylene, 0.6% polyethylene, 0.6% polypropylene, 0.4% ethylene-vinyl acetate copolymer, 0.6% polyethylene glycol, and 0.3% stearic acid;
[0017] The inorganic mixed powder is composed of the following raw materials in mass percentage: 20% modified SiC powder and the balance is made up of Cu powder with a laser particle size of D50=7-8μm;
[0018] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=5-5.5μm as a substrate, coating a 1μm thick tungsten film and a 1μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
[0019] Furthermore, the powder injection molding silicon carbide copper composite material comprises the following raw materials in mass percentage: 91.6% inorganic mixed powder, 6.4% polyoxymethylene, 0.8% polyethylene, 0.5% polystyrene, 0.4% dibutyl phthalate, and 0.3% stearic acid;
[0020] The inorganic mixed powder is composed of the following raw materials in mass percentage: 5% of modified SiC powder and the balance of Cu powder with laser particle size D50=5-6μm;
[0021] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=6-7μm as a substrate, coating a 1μm thick tungsten film and a 0.5μm thick copper film on the surface in sequence, and then keeping the temperature at 600°C for 2h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
[0022] Furthermore, the powder injection molding silicon carbide copper composite material comprises the following raw materials in percentage by mass: 89.6% inorganic mixed powder, 8.6% polyoxymethylene, 0.5% polyethylene, 0.6% polyamide, 0.4% polyethylene glycol, and 0.3% stearic acid;
[0023] The inorganic mixed powder is composed of the following raw materials in mass percentage: 10% of modified SiC powder and the balance of Cu powder with a laser particle size of D50=8-9 μm;
[0024] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=5-6μm as a substrate, coating a 1μm thick tungsten film and a 1.5μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
[0025] Furthermore, the powder injection molding silicon carbide copper composite material comprises the following raw materials in percentage by mass: 88% inorganic mixed powder, 0.2% microcrystalline wax, 9.5% polyoxymethylene, 1.3% polyethylene, 0.6% polyethylene glycol, and 0.4% zinc stearate;
[0026] The inorganic mixed powder is composed of the following raw materials in mass percentage: 15% of modified SiC powder and the balance of Cu powder with a laser particle size of D50 = 10-11 μm;
[0027] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=5-6μm as a substrate, coating a 1μm thick tungsten film and a 2μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
[0028] Furthermore, the powder injection molding silicon carbide copper composite material includes the following raw materials in mass percentage: 87.5% inorganic mixed powder, 5% paraffin wax, 2.5% microcrystalline wax, 3.8% polyethylene, 0.7% polystyrene, and 0.5% stearic acid;
[0029] The inorganic mixed powder is composed of the following raw materials in mass percentage: 30% of modified SiC powder and the balance of Cu powder with a laser particle size of D50=8-9 μm;
[0030] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=4-5μm as a substrate, coating a 0.8μm thick tungsten film and a 2μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
[0031] Furthermore, the powder injection molding silicon carbide copper composite material comprises the following raw materials in percentage by mass: 82% inorganic mixed powder, 7.25% paraffin wax, 3.65% polyoxymethylene, 5.4% polyethylene, 1% ethylene-vinyl acetate copolymer, and 0.7% zinc stearate;
[0032] The inorganic mixed powder is composed of the following raw materials in mass percentage: 40% of modified SiC powder and the balance of Cu powder with laser particle size D50=9-10 μm;
[0033] The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=1-2μm as a substrate, coating a 0.5μm thick tungsten film and a 1μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
[0034] The present invention further provides a method for preparing the powder injection molded silicon carbide copper composite material, based on the MIM molding process, using spherical copper powder and modified SiC powder mixed in proportion as raw materials, sintering to prepare a finished size SiC / Cu composite material, comprising the following steps:
[0035] S1: preparing modified SiC powder: plating tungsten on the surface of SiC by using one of the vacuum sputtering coating or vacuum evaporation coating methods in the physical vapor deposition method, the thickness of the tungsten layer is 0.5-1 μm, and after the tungsten plating is completed, the powder is further plated with a metal copper film by using one of the vacuum sputtering coating, evaporation coating, and chemical plating methods, the thickness of the copper layer is 0.5-2 μm;
[0036] S2: Mixing: Mix the modified SiC powder and the spherical Cu powder in a V-type mixer at a speed of 15 to 25 r / min for 2 to 4 hours;
[0037] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 1.5-2h. Mix evenly and then extrude and granulate to form feed;
[0038] S4: After powder injection molding, degreasing is performed to obtain a semi-finished product;
[0039] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours for thermal debinding, then heat it to 1050-1400°C and keep it at that temperature for 3-8 hours.
[0040] Furthermore, the degreasing adopts solvent immersion extraction degreasing or nitric acid / oxalic acid catalytic degreasing, the degreasing temperature is 60-140° C., and the degreasing time is 9-16 hours.
[0041] Beneficial effects of the present invention:
[0042] The invention sequentially plates a tungsten metal layer and a copper metal layer on the surface of silicon carbide powder to form a composite layer modified silicon carbide with silicon carbide as the core, the tungsten metal layer as the inner plating layer and the copper metal layer as the outer plating layer, and performs atomic crystallization and impurity removal treatment on the composite layer, thereby improving the wettability between silicon carbide and copper metal and avoiding the interface reaction between silicon carbide and copper at high temperature. The modified SiC powder can be directly used for preparing Si / Cu composite materials by powder injection molding method. The density of the sintered product is as high as more than 90%, and the microstructure metallographic diagram shows that the metal copper is evenly distributed and well combined with the SiC powder.
[0043] At the same time, the inventors can obtain a series of high thermal conductivity, high strength, and high wear resistance composite materials with different thermal expansion coefficients based on different proportions of SiC and Cu. These composite materials have high practicality and are suitable for chip packaging, communication module heat dissipation and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 This is a metallographic diagram of the silicon carbide copper composite material (modified SiC 5%+Cu 95%) prepared in Example 2;
[0046] Figure 2 This is a metallographic diagram of the silicon carbide copper composite material (modified SiC 10%+Cu 90%) prepared in Example 3. DETAILED DESCRIPTION
[0047] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0048] Example 1
[0049] A method for preparing a powder injection molded silicon carbide copper composite material comprises the following steps:
[0050] S1: Preparation of modified SiC powder: Using β-SiC (cubic silicon carbide) powder with a laser particle size of D50 = 5 to 5.5 μm as the substrate, a 1 μm tungsten metal layer is uniformly plated on the surface of the SiC powder using a vacuum sputtering coating device. The powder is continuously stirred and turned during the vacuum sputtering coating process to ensure uniform coating. The tungsten-plated SiC powder is copper-plated using a vacuum sputtering coating with a copper plating thickness of 1 μm. After copper plating, the powder is placed in a ceramic sagger and baked at 550°C in a hydrogen atmosphere furnace for 4 hours to make the crystal structure of the metal coating on the surface of the SiC powder regular and reduce the oxygen content and carbon content on the surface of the powder.
[0051] S2: Mixing: Modified SiC powder and spherical Cu powder (laser particle size D50 = 7-8 μm) are mixed at a mass ratio of modified SiC:Cu = 20:80. The mixing is carried out in a V-type mixer at a speed of 15 r / min for 2 h.
[0052] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is performed for 1.5h. Mix evenly and then extrude and granulate to form feed;
[0053] The feeding formula for internal mixing and granulation is as follows:
[0054]
[0055]
[0056] S4: After powder injection molding, degreasing is performed in an oxalic acid degreasing furnace at a degreasing temperature of 130°C for 12 hours to obtain a semi-finished product;
[0057] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours, perform thermal debinding, and then heat it to 1250°C and keep it at that temperature for 4 hours.
[0058] Example 2
[0059] A method for preparing a powder injection molded silicon carbide copper composite material comprises the following steps:
[0060] S1: Preparation of modified SiC powder: Using β-SiC (cubic silicon carbide) powder with a laser particle size of D50=6-7μm as the substrate, a 1μm tungsten metal layer is uniformly plated on the surface of the SiC powder using a vacuum sputtering coating device. The powder is continuously stirred and turned during the vacuum sputtering coating process to ensure uniform coating. The tungsten-plated SiC powder is copper-plated using chemical plating with a copper plating thickness of 0.5μm. After copper plating, the powder is cleaned and dried, and then placed in a ceramic sagger and baked at 600℃ in a hydrogen atmosphere furnace for 2h to make the crystal structure of the metal coating on the surface of the SiC powder regular and reduce the oxygen content and carbon content on the surface of the powder.
[0061] S2: Mixing: Modified SiC powder and spherical Cu powder (laser particle size D50 = 5-6 μm) are mixed at a mass ratio of modified SiC:Cu = 5:95. The mixing is carried out in a V-type mixer at a speed of 15 r / min for 4 hours.
[0062] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 2h. Mix evenly and then extrude and granulate to form feed;
[0063] The feeding formula for internal mixing and granulation is as follows:
[0064]
[0065] S4: After powder injection molding, degreasing is performed in an oxalic acid degreasing furnace at a degreasing temperature of 130°C for 9 hours to obtain a semi-finished product;
[0066] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours, perform thermal debinding, and then heat it to 1050°C and keep it at that temperature for 4 hours.
[0067] Example 3
[0068] A method for preparing a powder injection molded silicon carbide copper composite material comprises the following steps:
[0069] S1: Preparation of modified SiC powder: Using β-SiC (cubic silicon carbide) powder with a laser particle size of D50 = 5-6 μm as the substrate, a 1 μm tungsten metal layer is uniformly plated on the surface of the SiC powder using a vacuum sputtering coating device. The powder is continuously stirred and turned during the vacuum sputtering coating process to ensure uniform coating. The tungsten-plated SiC powder is plated with copper using chemical plating with a thickness of 1.5 μm. After copper plating, the powder is cleaned and dried, and then placed in a ceramic sagger and baked at 550°C in a hydrogen atmosphere furnace for 4 hours to make the crystal structure of the metal coating on the surface of the SiC powder regular and reduce the oxygen content and carbon content on the surface of the powder.
[0070] S2: Mixing: Modified SiC powder and spherical Cu powder (laser particle size D50 = 8-9 μm) are mixed at a mass ratio of modified SiC:Cu = 10:90. The mixing is carried out in a V-type mixer at a speed of 15 r / min for 3 h.
[0071] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 2h. Mix evenly and then extrude and granulate to form feed;
[0072] The feeding formula for internal mixing and granulation is as follows:
[0073]
[0074] S4: After powder injection molding, degreasing is performed in an oxalic acid degreasing furnace at a degreasing temperature of 130°C for 16 hours to obtain a semi-finished product;
[0075] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours, perform thermal debinding, and then heat it to 1070°C and keep it at that temperature for 3 hours.
[0076] Example 4
[0077] A method for preparing a powder injection molded silicon carbide copper composite material comprises the following steps:
[0078] S1: Preparation of modified SiC powder: Using β-SiC (cubic silicon carbide) powder with a laser particle size of D50 = 5-6 μm as the substrate, a 1 μm tungsten metal layer is uniformly plated on the surface of the SiC powder using a vacuum sputtering coating device. The powder is continuously stirred and turned during the vacuum sputtering coating process to make the coating uniform; the tungsten-plated SiC powder is copper-plated using a vacuum sputtering coating with a copper plating thickness of 2 μm. After copper plating, the powder is placed in a ceramic sagger and baked at 550°C in a hydrogen atmosphere furnace for 4 hours to make the crystal structure of the metal coating on the surface of the SiC powder regular and reduce the oxygen content and carbon content on the surface of the powder;
[0079] S2: Mixing: Modified SiC powder and spherical Cu powder (laser particle size D50 = 10-11 μm) are mixed at a mass ratio of modified SiC:Cu = 15:85. The mixing is carried out in a V-type mixer at a speed of 15 r / min for 4 hours.
[0080] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 2h. Mix evenly and then extrude and granulate to form feed;
[0081] The feeding formula for internal mixing and granulation is as follows:
[0082]
[0083] S4: After powder injection molding, degreasing is performed in an oxalic acid degreasing furnace at a degreasing temperature of 135°C for 12 hours to obtain a semi-finished product;
[0084] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours, perform thermal debinding, and then heat it to 1160°C and keep it at that temperature for 3 hours.
[0085] Example 5
[0086] A method for preparing a powder injection molded silicon carbide copper composite material comprises the following steps:
[0087] S1: Preparation of modified SiC powder: Using β-SiC (cubic silicon carbide) powder with a laser particle size of D50 = 4-5 μm as the substrate, a 0.8 μm tungsten metal layer is uniformly plated on the surface of the SiC powder using a vacuum sputtering coating device. The powder is continuously stirred and turned during the vacuum sputtering coating process to ensure uniform coating. The tungsten-plated SiC powder is copper-plated using a vacuum sputtering coating with a copper plating thickness of 2 μm. After copper plating, the powder is placed in a ceramic sagger and baked at 550°C in a hydrogen atmosphere furnace for 4 hours to make the crystal structure of the metal coating on the surface of the SiC powder regular and reduce the oxygen content and carbon content on the surface of the powder.
[0088] S2: Mixing: Modified SiC powder and spherical Cu powder (laser particle size D50 = 8-9 μm) are mixed at a mass ratio of modified SiC:Cu = 30:70. The mixing is carried out in a V-type mixer at a speed of 15 r / min for 4 hours.
[0089] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 2h. Mix evenly and then extrude and granulate to form feed;
[0090] The feeding formula for internal mixing and granulation is as follows:
[0091]
[0092] S4: After powder injection molding, solvent extraction degreasing is performed using a limonene + dipentene mixed solution (mass ratio 1:1) at a solvent temperature of 60°C and a degreasing time of 12 hours to obtain a semi-finished product;
[0093] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours, perform thermal debinding, and then heat it to 1310°C and keep it at that temperature for 6 hours.
[0094] Example 6
[0095] A method for preparing a powder injection molded silicon carbide copper composite material comprises the following steps:
[0096] S1: Preparation of modified SiC powder: Using β-SiC (cubic silicon carbide) powder with a laser particle size of D50 = 1-2 μm as the substrate, a 0.5 μm tungsten metal layer is uniformly plated on the surface of the SiC powder using a vacuum sputtering coating device. The powder is continuously stirred and turned during the vacuum sputtering coating process to make the coating uniform; the tungsten-plated SiC powder is copper-plated using a vacuum sputtering coating with a copper plating thickness of 1 μm. After copper plating, the powder is placed in a ceramic sagger and baked at 550°C in a hydrogen atmosphere furnace for 4 hours to make the crystal structure of the metal coating on the surface of the SiC powder regular and reduce the oxygen content and carbon content on the surface of the powder;
[0097] S2: Mixing: Modified SiC powder and spherical Cu powder (laser particle size D50 = 9-10 μm) are mixed at a mass ratio of modified SiC:Cu = 40:60. The mixing is carried out in a V-type mixer at a speed of 25 r / min for 4 hours.
[0098] S3: Banburying granulation: add a certain amount of other high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 2h. Mix evenly and then extrude and granulate to form feed;
[0099] The feeding formula for internal mixing and granulation is as follows:
[0100]
[0101] S4: After powder injection molding, degreasing is performed in an oxalic acid degreasing furnace at a degreasing temperature of 140°C for 12 hours to obtain a semi-finished product;
[0102] S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours, perform thermal debinding, and then heat it to 1400°C and keep it at that temperature for 8 hours.
[0103] Comparative Example 1
[0104] The same as Example 1, except that: the SiC powder is not modified, and β-SiC (cubic silicon carbide) powder with a laser particle size D50=5-5.5 μm is directly mixed with the spherical Cu powder.
[0105] The results showed that the sintered density was very low, the Cu component was partially precipitated out of the surface, and there was almost no shrinkage and strength.
[0106] Comparative Example 2
[0107] The same as Example 2, except that: β-SiC (cubic silicon carbide) powder with a laser particle size D50=6-7μm is used as the substrate, copper plating is performed by chemical plating, the copper plating thickness is 0.5μm, and the SiC powder is not treated with hydrogen after copper plating.
[0108] Comparative Example 3
[0109] The same as Example 3, except that: the SiC powder is not modified, and β-SiC (cubic silicon carbide) powder with a laser particle size D50=5-6 μm is directly mixed with the spherical Cu powder.
[0110] The results showed that the sintered density was very low, the Cu component was partially precipitated out of the surface, and there was almost no shrinkage and strength.
[0111] The following table lists the physical and chemical properties of the SiC / Cu composite materials prepared in various embodiments and comparative examples:
[0112]
[0113] As can be seen from the above table, the SiC / Cu composite materials sintered in Examples 1 to 6 have good density, with a density of more than 90%, and according to different proportions of SiC and Cu, a series of high thermal conductivity, high strength, and high wear-resistant materials with different thermal expansion coefficients can be obtained. At the same time, by comparing the data of Example 1 and Comparative Example 1, Example 3 and Comparative Example 3, it can be seen that plating metal tungsten and metal copper on the surface of β-SiC powder can greatly improve the sintering density and density of SiC / Cu composite materials, which shows that the wettability between silicon carbide and copper metal is improved by modifying the tungsten-copper composite metal layer, and at the same time, silicon carbide is prevented from reacting with copper at high temperature; by observing the data of Example 2 and Comparative Example 2, it can be seen that plating metal tungsten on the surface of β-SiC powder in advance also improves the sintering density and density of SiC / Cu composite materials to a certain extent, which shows that the inner tungsten metal layer has a certain synergistic effect on the outer copper metal layer, further improving the compact performance. While Comparative Example 1 uses unmodified SiC powder as the sintering raw material, it cannot be densified and cannot obtain qualified sintered products. However, Comparative Example 3 uses unmodified SiC powder as the sintering raw material to obtain dense products, indicating that the ratio of SiC to Cu also has an important influence on the density. The amount of SiC in the composite system is negatively correlated with the sintering density and compactness. When the amount of SiC in the composite system is lower, the sintering density and compactness are higher, and vice versa.
[0114] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0115] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A powder injection molded silicon carbide copper composite material, characterized in that: The invention comprises the following raw materials in percentage by mass: 82-91.6% of inorganic mixed powder, 0-7.25% of paraffin wax, 0-2.5% of microcrystalline wax, 0-11.2% of polyoxymethylene, 0.5-5.4% of polyethylene, 0-0.6% of polypropylene, 0-1% of ethylene-vinyl acetate copolymer, 0-0.6% of polyamide, 0-0.6% of polyethylene glycol, 0-0.7% of polystyrene, 0-0.4% of dibutyl phthalate and 0.3-0.7% of surfactant; The inorganic mixed powder is composed of the following raw materials in mass percentage: 5-40% of modified SiC powder and the balance of Cu powder with laser particle size D50=5-11 μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=1-7μm as a substrate, coating a tungsten film with a thickness of 0.5-1μm and a copper film with a thickness of 0.5-2μm on the surface of the substrate in sequence, and then maintaining the temperature at 550-600°C in a hydrogen atmosphere for 2-8h to obtain tungsten / copper modified SiC powder.
2. The powder injection molding silicon carbide copper composite material according to claim 1, characterized in that: The surfactant is one of stearic acid or zinc stearate.
3. The powder injection molding silicon carbide copper composite material according to claim 2, characterized in that: The raw materials include the following by mass percentage: 86.1% inorganic mixed powder, 0.2% paraffin wax, 11.2% polyoxymethylene, 0.6% polyethylene, 0.6% polypropylene, 0.4% ethylene-vinyl acetate copolymer, 0.6% polyethylene glycol, and 0.3% stearic acid; The inorganic mixed powder is composed of the following raw materials in mass percentage: 20% modified SiC powder and the balance is made up of Cu powder with a laser particle size of D50=7-8μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=5-5.5μm as a substrate, coating a 1μm thick tungsten film and a 1μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
4. The powder injection molding silicon carbide copper composite material according to claim 2, characterized in that: The raw materials include the following mass percentages: 91.6% inorganic mixed powder, 6.4% polyoxymethylene, 0.8% polyethylene, 0.5% polystyrene, 0.4% dibutyl phthalate, and 0.3% stearic acid; The inorganic mixed powder is composed of the following raw materials in mass percentage: 5% of modified SiC powder and the balance of Cu powder with laser particle size D50=5-6μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=6-7μm as a substrate, coating a 1μm thick tungsten film and a 0.5μm thick copper film on the surface in sequence, and then keeping the temperature at 600°C for 2h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
5. The powder injection molding silicon carbide copper composite material according to claim 2, characterized in that: The raw materials include the following mass percentages: 89.6% inorganic mixed powder, 8.6% polyoxymethylene, 0.5% polyethylene, 0.6% polyamide, 0.4% polyethylene glycol, and 0.3% stearic acid; The inorganic mixed powder is composed of the following raw materials in mass percentage: 10% of modified SiC powder and the balance of Cu powder with a laser particle size of D50=8-9 μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=5-6μm as a substrate, coating a 1μm thick tungsten film and a 1.5μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
6. The powder injection molding silicon carbide copper composite material according to claim 2, characterized in that: The raw materials include the following mass percentages: 88% inorganic mixed powder, 0.2% microcrystalline wax, 9.5% polyoxymethylene, 1.3% polyethylene, 0.6% polyethylene glycol, and 0.4% zinc stearate; The inorganic mixed powder is composed of the following raw materials in mass percentage: 15% of modified SiC powder and the balance of Cu powder with a laser particle size of D50 = 10-11 μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=5-6μm as a substrate, coating a 1μm thick tungsten film and a 2μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
7. The powder injection molding silicon carbide copper composite material according to claim 2, characterized in that: The raw materials include the following mass percentages: 87.5% inorganic mixed powder, 5% paraffin wax, 2.5% microcrystalline wax, 3.8% polyethylene, 0.7% polystyrene, and 0.5% stearic acid; The inorganic mixed powder is composed of the following raw materials in mass percentage: 30% of modified SiC powder and the balance of Cu powder with a laser particle size of D50=8-9 μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=4-5μm as a substrate, coating a 0.8μm thick tungsten film and a 2μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
8. The powder injection molding silicon carbide copper composite material according to claim 2, characterized in that: The raw materials include the following mass percentages: 82% inorganic mixed powder, 7.25% paraffin wax, 3.65% polyoxymethylene, 5.4% polyethylene, 1% ethylene-vinyl acetate copolymer, and 0.7% zinc stearate; The inorganic mixed powder is composed of the following raw materials in mass percentage: 40% of modified SiC powder and the balance of Cu powder with laser particle size D50=9-10 μm; The preparation method of the modified SiC powder is as follows: using β-SiC powder with a laser particle size D50=1-2μm as a substrate, coating a 0.5μm thick tungsten film and a 1μm thick copper film on the surface in sequence, and then keeping the temperature at 550°C for 4h in a hydrogen atmosphere to obtain tungsten / copper modified SiC powder.
9. A method for preparing a powder injection molded silicon carbide copper composite material according to any one of claims 1 to 8, characterized in that: Based on the MIM molding process, spherical copper powder and modified SiC powder are mixed in proportion as raw materials, and sintered to prepare SiC / Cu composite materials of finished size, including the following steps: S1: preparing modified SiC powder: plating tungsten on the surface of SiC, the thickness of the tungsten layer is 0.5-1 μm, and after the tungsten plating is completed, a layer of metal copper film is plated, the thickness of the copper layer is 0.5-2 μm; S2: Mixing: Mix the modified SiC powder and the spherical Cu powder in a V-type mixer at a speed of 15 to 25 r / min for 2 to 4 hours; S3: Banburying granulation: add a certain amount of high molecular organic matter to the mixed powder, and add it to the banburying tank. The temperature of the banburying tank is 180-185℃, the speed is 15r / min, and the banburying is carried out for 1.5-2h. Mix evenly and then extrude and granulate to form feed; S4: After powder injection molding, degreasing is performed to obtain a semi-finished product; S5: Sintering: In a hydrogen atmosphere, heat the semi-finished product to 600°C at a rate of 2.5°C / min and keep it at that temperature for 4 hours for thermal debinding, then heat it to 1050-1400°C and keep it at that temperature for 3-8 hours.
10. The method for preparing a powder injection molded silicon carbide copper composite material according to claim 9, characterized in that: The degreasing is carried out by solvent immersion extraction degreasing or nitric acid / oxalic acid catalytic degreasing, the degreasing temperature is 60-140° C., and the degreasing time is 9-16 hours.