A method for preparing glue-free bamboo-based filament board

By combining steam explosion and low-temperature plasma treatment, the molecular structure of bamboo fiber is regulated to produce high-strength, environmentally friendly, glue-free bamboo-based fiberboard, solving the problems of formaldehyde pollution and low production efficiency of traditional bamboo-based engineered wood products.

CN118107029BActive Publication Date: 2024-11-22SOUTHWEST FORESTRY UNIVERSITY

Patent Information

Application Number
CN202410400866.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-11-22
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

The aldehyde-based adhesives used in existing bamboo-based engineered wood products manufacturing methods cause formaldehyde pollution, and glue-free solutions suffer from low production efficiency, high cost, and unstable products, making it difficult to produce high-strength, environmentally friendly glue-free bamboo fiberboard.

Method used

Bamboo fibers are treated with steam explosion and combined with low-temperature plasma treatment to regulate the molecular structure of bamboo fibers under different atmospheres, forming a micro-nano porous structure, thereby achieving self-bonding of bamboo fibers and preparing glue-free bamboo-based fiberboard.

Benefits of technology

This technology achieves high internal bond strength, low brittleness, low moisture absorption, and environmental friendliness in glue-free bamboo-based fiberboard, reducing production costs and meeting green environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118107029B_ABST
    Figure CN118107029B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of bamboo-based artificial board preparation, and discloses a method for preparing a glue-free bamboo-based filament board, which is prepared by hot pressing bamboo-based filaments, wherein the bamboo-based filaments are subjected to plasma treatment, and the bamboo-based filaments are obtained by steam explosion treatment, and the length of the bamboo-based filaments is 6 to 10 cm and the width is 50 to 150 μm; the plasma treatment is low-temperature plasma treatment, the discharge power is 80 to 500 W, and the total treatment time is 220 to 600 s. The steps of the plasma treatment include the first stage to the third stage, and the plasma treatment is carried out in a mixed gas of argon / helium and ammonia / nitrogen respectively. The method for preparing the glue-free bamboo-based filament board of this case has at least the advantages of low weight, high strength, high internal bonding strength, non-toxicity, and green environmental protection, and the preparation cost is relatively low, and mass production can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of bamboo-based artificial boards, and more specifically, to a method for preparing a glue-free bamboo-based filament board. The method obtains bamboo filaments by steam explosion, and further performs low-temperature plasma treatment on the bamboo filaments to achieve self-adhesion of the bamboo filaments, thereby preparing the glue-free bamboo-based filament board. Background Art

[0002] Bamboo is an important biomass material that has significant ecological, economic and social benefits because of its green, low-carbon, fast-growing, renewable and degradable nature.

[0003] Bamboo-based artificial board is a kind of board made from bamboo. The traditional preparation method of bamboo-based artificial board includes the steps of bamboo separation, drying, impregnation, paving, hot pressing, etc. The adhesives used in the above preparation methods are mostly aldehyde adhesives, so the free formaldehyde generated during the processing and subsequent use of the products will cause secondary pollution, making the products and their preparation methods not meet the current requirements for green environmental protection.

[0004] In order to make bamboo-based artificial boards and their preparation methods meet the requirements of green environmental protection, the prior art proposes a technical solution for non-glue bamboo-based artificial boards. Non-glue artificial boards are made of bamboo fibers as raw materials, and the reaction activity of bamboo fibers is improved by oxidation bonding, enzyme activation, acid-catalyzed polycondensation and / or alkali activation of bamboo fibers, so that they can be combined into boards only by the role of lignin, hemicellulose and cellulose in bamboo fiber materials during hot pressing.

[0005] For example, in the invention patent application with publication number CN 1412092 and titled “Deformed Straw Material and Its Use”, a method for preparing straw modified material by hot pressing after inoculating straw with steam explosion and then activating the straw material by solid-state fermentation with Phanerochaete chrysosporium was proposed. However, this method has a low production efficiency of the pressing plate due to the long growth cycle of microorganisms, and the uneven distribution of laccase activity can easily lead to product instability.

[0006] For example, in the invention patent application with the publication number CN 107009478A and the name "A method for enhancing the interfacial bonding ability of fiberboard by treating wood fiber with plasma", a technical solution for treating wood fiber with plasma to improve its interfacial activity is proposed. Specifically, the interfacial bonding effect of the wood fiber and lignin blend treated with plasma is good, and the internal bonding strength is much higher than that of the board formed by hot pressing of untreated wood fiber and lignin. Compared with the board formed by hot pressing of untreated wood fiber and lignin, the dimensional stability and durability of the environmentally friendly fiberboard made of wood fiber and lignin treated with plasma are also improved to a certain extent. The patent application also points out that the wood surface is coarsened and the surface is severely etched after plasma treatment, and the surface free energy of wood fiber is increased and the surface wetting angle is reduced, which are all conducive to the improvement of the interfacial bonding ability of wood fiber and lignin. However, the above scheme can only improve the interfacial bonding ability of wood fiber, but when preparing wood-based fiberboard, 8 to 12% by mass of lignin still needs to be added as a binder, and the self-bonding of wood fiber cannot be achieved. At the same time, the addition of industrial lignin, the use of plasma treatment in a high-temperature environment, and the plasma treatment in a single oxygen atmosphere all greatly increase the cost of product preparation.

[0007] In summary, a method for preparing a glue-free bamboo-based filament board using bamboo as a material is needed to meet the market demand for environmentally friendly, safe formaldehyde-free materials while having a relatively low production cost. Summary of the invention

[0008] The technical purpose of this case is to overcome at least one of the above-mentioned technical problems, and to provide a method for preparing a glue-free bamboo-based filament board. The method obtains bamboo filaments by steam explosion, and further performs low-temperature plasma treatment on the bamboo filaments to achieve self-adhesion of the bamboo filaments, thereby preparing a glue-free bamboo-based filament board.

[0009] In one aspect of the present invention, a method for preparing a non-glue bamboo-based filament board is provided, wherein a first-state bamboo-based filament is obtained by steam explosion treatment, wherein the first-state bamboo-based filament has a length of 6 to 10 cm and a width of 50 to 150 μm, and then the first-state bamboo-based filament is subjected to low-temperature plasma treatment to obtain a second-state bamboo-based filament, and finally the second-state bamboo-based filament is subjected to hot pressing treatment to prepare the non-glue bamboo-based filament board;

[0010] The discharge power of the low-temperature plasma treatment is 80 to 500 W, and the total treatment time is 220 to 600 s. The low-temperature plasma treatment includes the first stage to the third stage. In the first stage, the plasma treatment is carried out in a mixed gas of carbon dioxide / oxygen. In the second stage, the plasma treatment is carried out in a mixed gas of argon / helium. In the third stage, the plasma treatment is carried out in a mixed gas of ammonia / nitrogen.

[0011] In the theory of the prior art, the high temperature and pressure provided by the outside during the hot pressing process can make the lignin melt and flow, the cellulose and lignin themselves and each other hydrogen bond, and the hemicellulose degrade and form a polymer with the lignin, which makes the bamboo / wood-based fiber have the possibility of self-bonding. In other words, it is possible to prepare a glue-free bamboo / wood-based fiberboard by utilizing the self-bonding ability between bamboo / wood-based fibers without adding auxiliary binders such as adhesives or industrial lignin. However, in actual operation, glue-free bamboo / wood-based fiberboard is rarely seen. On the one hand, the self-bonding force formed by the high temperature and pressure of the hot pressing step is small and it is difficult to form sufficient internal bonding strength. On the other hand, since this scheme is only applicable to short fibers, the prepared board is relatively brittle.

[0012] In this case, the above method is used to treat the lignin and cellulose in bamboo-based filaments through steam explosion, combined with low-temperature plasma treatment in three stages and different atmospheres, so as to directionally regulate the molecular structure of lignin and cellulose in bamboo-based filaments and the types and contents of their surface functional groups. Specifically, the lignin macromolecules migrate from the bamboo-based filaments during the steam explosion process and depolymerize into lignin units with low polycondensation. Subsequently, the low-temperature plasma directional induction regulation introduces relatively high content of oxygen-containing and nitrogen-containing functional groups such as -OH, -CHO, -NH2 and -CONH2 into the cellulose molecular chain of the bamboo fiber. At the same time, under the induction of plasma, the oxygen-containing and nitrogen-containing functional groups on the cellulose molecular chain are connected to the low polycondensation lignin units, as well as aldehyde amine condensation, carboxyl hydroxy esterification, and aldol condensation reactions, thereby improving the bonding strength and internal bonding strength of the glue-free bamboo-based filament board. The low polycondensation lignin formed by non-polycondensation and depolymerization can produce covalent self-bonding (self-crosslinking) during the hot pressing treatment, which makes the lignin have a bonding effect.

[0013] The aforementioned comparative document CN107009478A can form etching on the surface of wood fibers, thereby improving the interfacial properties of wood fibers. After low-temperature plasma treatment in this case, the bamboo-based filaments form a micro-nano porous structure. The loose micro-nano porous structure can improve the interfacial properties of the bamboo-based filaments, increase its surface free energy, and reduce the surface wetting angle. More importantly, the micro-nano porous bamboo-based filaments can penetrate and entangle with each other. The potential "mechanical interlocking" physical synergistic binding effect generated by the interpenetration and entanglement of bamboo-based filaments can form a relatively strong binding force, which is much greater than the binding force formed by the simple entanglement and weaving of the filaments. The interpenetration and entanglement of bamboo-based filaments improves the internal bonding strength of the glue-free bamboo-based filament board in this case.

[0014] Additionally, as mentioned above, the low-temperature plasma treatment process of this case can effectively act on bamboo-based filaments with a large aspect ratio. The use of bamboo-based filaments with a large aspect ratio can naturally improve the brittleness of the glue-free board, improve the mechanical strength of the product, and reduce the hygroscopicity of the glue-free bamboo-based filament board. However, the existing technology can only use powdered bamboo / wood fibers to prepare glue-free boards, so the prepared glue-free boards are brittle and hygroscopic.

[0015] Additionally, the micro-nano porous bamboo-based filaments can also reduce the density of the glue bamboo-based filament board of this case to a certain extent, making it have the advantages of light weight, high strength, non-toxic and environmentally friendly.

[0016] As a preferred embodiment, in the carbon dioxide / oxygen mixed gas, the ratio of carbon dioxide to oxygen is 2:8 to 8:2.

[0017] As a preferred implementation, in the argon / helium mixed gas, the ratio of argon to helium is 1:1.

[0018] As a preferred embodiment, in the ammonia / nitrogen mixed gas, the ratio of ammonia to nitrogen is 1:9 to 9:1.

[0019] As a preferred embodiment, the discharge power of the plasma treatment is 300-500 W and the treatment time is 100-150 s.

[0020] As a preferred implementation, the processing time of the first stage is 160 to 200 s, the processing time of the second stage is 60 to 100 s, and the processing time of the third stage is 60 to 100 s.

[0021] As a preferred embodiment, the low-temperature plasma of the plasma treatment includes at least one of corona discharge, glow discharge, dielectric barrier discharge or radio frequency plasma.

[0022] As a preferred embodiment, the plasma treatment is radio frequency discharge treatment alone, dielectric barrier discharge treatment alone, or radio frequency discharge-dielectric barrier discharge combined treatment.

[0023] As a preferred embodiment, the steam explosion pressure is 1-4 MPa, the temperature is 120-240° C., and the pressure holding time is 30-300 s.

[0024] As a preferred embodiment, before the steam explosion treatment, the bamboo strips are pretreated; the pretreatment is that the bamboo strips are soaked in hot water at a temperature of 80 to 100° C. for 4 to 8 hours, and then soaked in cold water at room temperature for 24 to 48 hours.

[0025] As a preferred embodiment, before the plasma treatment, the bamboo-based filaments are ultrasonically cleaned and dispersed, and then the bamboo-based filaments are dried to a moisture content of 3 to 12%.

[0026] As a preferred embodiment, the temperature of the hot pressing treatment is 190-250° C., the pressure is 0.5-2.5 MPa, and the time is 5-15 min to obtain the glue-free bamboo-based filament board.

[0027] In summary, the preparation method of the glue-free bamboo-based filament board of this case has at least the advantages of low weight, high strength, high internal bonding strength, non-toxicity, and green environmental protection, and the preparation cost is relatively low and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative labor.

[0029] Figure 1 This is a photo of the glue-free bamboo-based filament board according to an embodiment of the present application. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.

[0031] A method for preparing a non-glue bamboo-based filament board comprises the following process steps in sequence.

[0032] (A) Obtaining bamboo strips.

[0033] The main bamboo poles are taken and decomposed into bamboo strips by a decomposing machine. The bamboo used is preferably clumping bamboo or scattered bamboo with a diameter of not less than 2 cm and a growth period of more than 2 years.

[0034] (B) Pretreatment of bamboo strips.

[0035] The bamboo strips obtained by deflocculent treatment are placed in hot water at a temperature of 80 to 100° C. and soaked for 4 to 8 hours, and then soaked in cold water for 24 to 48 hours.

[0036] (C) Steam explosion treatment of bamboo strips.

[0037] The pretreated bamboo strips are placed in a steam explosion device for defibration treatment to obtain bamboo-based filaments with a length of 6 to 10 cm and a width of 50 to 150 μm. The pressure of the steam explosion device is controlled to be 1 to 4 MPa and the temperature to be 120 to 240° C. The pressure of the steam explosion treatment is maintained for 30 to 300 seconds.

[0038] (D) Dispersion treatment of bamboo-based filaments.

[0039] The bamboo-based filaments are ultrasonically cleaned and dispersed in an ultrasonic disperser for 10 to 30 minutes, and then the cleaned and dispersed bamboo-based filaments are dried to a moisture content of 3 to 12%. Preferably, 500 to 800W microwaves are used to dry the bamboo-based filaments for 30 to 120 seconds.

[0040] (E) Low-temperature plasma treatment of dried bamboo-based filaments.

[0041] The dried bamboo-based filaments are placed in a low-temperature plasma treatment device for low-temperature plasma treatment including the first to third stages, the discharge power of the low-temperature plasma treatment is 80-500W, the total treatment time is 220-600s, and the temperature in the reactor is 35-55°C. The low-temperature plasma treatment in the first stage (E1) is carried out in a mixed gas of carbon dioxide / oxygen, the low-temperature plasma treatment in the second stage (E2) is carried out in a mixed gas of argon / helium, and the low-temperature plasma treatment in the third stage (E3) is carried out in a mixed gas of ammonia / nitrogen. Preferably, the ratio of carbon dioxide to oxygen is 2:8 to 8:2, the ratio of argon to helium is 1:1, and the ratio of ammonia to nitrogen is 1:9 to 9:1.

[0042] The inventor creatively discovered that, compared with a single oxygen atmosphere, the gases mixed in the above ratio can obtain the target type of groups and content, thereby obtaining a relatively good bamboo-based fiber bonding effect. In particular, in the two stages, the synergistic effect of nitrogen and helium can obtain a relatively large number of nitrogen-containing functional groups.

[0043] Additionally, the introduction of carbon dioxide gas can reduce the processing cost of the low-temperature plasma processing to a certain extent.

[0044] The low temperature plasma of the plasma treatment includes at least one of corona discharge, glow discharge, dielectric barrier discharge or radio frequency plasma.

[0045] (F) Heat pressing treatment of bamboo-based filaments.

[0046] The bamboo-based filaments are placed in a hot press with a mold for shaping, or placed on a conveyor belt of a continuous hot press for shaping. The temperature of the hot press treatment is 190-250°C, the pressure is 0.5-2.5 MPa, and the time is 5-15 minutes. Finally, the bamboo-based filaments are obtained. Figure 1 The glue-free bamboo-based filament board shown.

[0047] Example 1: The pretreated bamboo strips were placed in a steam explosion device for defibration treatment to obtain bamboo-based filaments. The pressure of the steam explosion device was controlled to be 1 MPa and the temperature to be 120° C. The pressure was maintained for 200 seconds during the steam explosion treatment.

[0048] The bamboo-based filaments were ultrasonically cleaned and dispersed in an ultrasonic disperser for 10 minutes, and then the cleaned and dispersed bamboo-based filaments were microwave dried under the process conditions of 500W and 60s to a moisture content of 3-12%.

[0049] The dried bamboo-based filaments were placed in a plasma treatment device for low-temperature plasma treatment including the first to third stages, with a discharge power of 80W and a total treatment time of 280s. Among them, the low-temperature plasma is a radio frequency discharge-dielectric barrier discharge combined treatment; the plasma treatment in the first stage (E1) was carried out in a carbon dioxide / oxygen mixed gas, with a carbon dioxide to oxygen ratio of 1:1, and a treatment time of 160s; the plasma treatment in the second stage (E2) was carried out in an argon / helium mixed gas, with an argon to helium ratio of 1:1, and a treatment time of 60s; the plasma treatment in the third stage (E3) was carried out in an ammonia / nitrogen mixed gas, with an ammonia to nitrogen ratio of 1:1, and a treatment time of 60s.

[0050] The bamboo-based filaments were placed on a conveyor belt of a continuous hot press for finishing and forming, and the hot pressing temperature was 200° C., the pressure was 0.5 MPa, and the time was 5 min. The obtained glue-free bamboo-based filament board was recorded as S1.

[0051] Example 2: The difference between Example 2 and Example 1 is that the pressure of the steam explosion equipment is controlled to be 2MPa, the temperature is 190°C, and the pressure of the steam explosion treatment is maintained for 200s; the discharge power of the plasma treatment is 100W, the total treatment time is 340s, and the treatment time of the three stages is 180s, 80s, and 80s respectively; the temperature of the hot pressing treatment is 200°C, the pressure is 1.5MPa, and the time is 10min. The obtained glue-free bamboo-based filament board is recorded as S2.

[0052] Example 3: The difference between Example 3 and Example 2 is that the discharge power of the plasma treatment is 200 W and the treatment time is 340 s. The obtained glue-free bamboo-based filament board is denoted as S3.

[0053] Example 4: The difference between Example 4 and Example 3 is that the discharge power of the plasma treatment is 300 W and the treatment time is 340 s. The obtained glue-free bamboo-based filament board is recorded as S4.

[0054] Example 5: The difference between Example 5 and Example 4 is that the pressure of the steam explosion equipment is controlled to be 3.5 MPa, the temperature is 220° C., and the pressure of the steam explosion treatment is maintained for 200 seconds. The obtained glue-free bamboo-based filament board is recorded as S5.

[0055] Example 6: The difference between Example 6 and Example 5 is that the ratio of carbon dioxide to oxygen in the first stage (E1) is 2:8, the ratio of argon to helium in the second stage (E2) is 1:1, and the ratio of ammonia to nitrogen in the third stage (E3) is 1:9. The obtained glue-free bamboo-based filament board is recorded as S6.

[0056] Example 7: The difference between Example 7 and Example 5 is that the ratio of carbon dioxide to oxygen in the first stage (E1) is 8:2, the ratio of argon to helium in the second stage (E2) is 1:1, and the ratio of ammonia to nitrogen in the third stage (E3) is 8:2. The obtained glue-free bamboo-based filament board is recorded as S7.

[0057] Example 8: The difference between Example 8 and Example 5 is that the ratio of carbon dioxide to oxygen in the first stage (E1) is 8:2, the ratio of argon to helium in the second stage (E2) is 1:1, and the ratio of ammonia to nitrogen in the third stage (E3) is 9:1. The obtained glue-free bamboo-based filament board is recorded as S8.

[0058] Example 9: The difference between Example 9 and Example 7 is that the temperature of the hot pressing treatment is 220° C., the pressure is 1.5 MPa, and the time is 10 min. The obtained glue-free bamboo-based filament board is denoted as S9.

[0059] Example 10: The difference between Example 10 and Example 7 is that the temperature of the hot pressing treatment is 220° C., the pressure is 3 MPa, and the time is 10 min. The obtained glue-free bamboo-based filament board is recorded as S10.

[0060] Example 11: The difference between Example 11 and Example 10 is that the discharge power of the plasma treatment is 500 W and the treatment time is 120 s. The obtained glue-free bamboo-based filament board is denoted as S11.

[0061] Table 1 shows the process conditions of Examples 1 to 11.

[0062] Table 1. Process conditions of Examples 1 to 11

[0063]

[0064]

[0065] Comparative Example 1: A bamboo-based fiber board containing glue was prepared by the method of the prior art. Specifically, bamboo strips were used to obtain bamboo-based fibers by the means of the prior art, and then the bamboo-based fibers were dried to a moisture content of 3-12% by microwave drying under the process conditions of 500W and 60s, and then commercial urea-formaldehyde resin was sprayed on the bamboo-based fibers to apply glue, and the amount of glue applied was 100kg / m 3 Finally, the sizing bamboo-based filaments were placed in a hot press at a temperature of 200°C and a pressure of 1.5 MPa for 10 min to obtain a urea-formaldehyde resin bamboo-based filament board, which was recorded as S12.

[0066] Comparative Example 2: Using the technical solution described in CN107009478A, the treatment object is changed to bamboo-based filaments with a moisture content of 12-16% obtained by drying in a drying kiln. Specifically, the discharge power of the plasma treatment is 650W, the treatment time is 180s, the temperature in the reactor is 200-240°C, and the gas is oxygen. The bamboo-based filaments after the plasma treatment are subjected to a hot pressing treatment under the process conditions of 220°C, 3MPa, and 10min, but no industrial lignin is added before the hot pressing treatment, and finally a non-glue bamboo-based filament board is obtained.

[0067] Table 2 shows the physical and chemical properties of the bamboo-based filament boards of Examples 1 to 11 and Comparative Examples 1 to 2.

[0068] Table 2. Physical and chemical properties of bamboo-based fiber boards of Examples 1 to 11 and Comparative Examples 1 to 2

[0069]

[0070]

[0071] The above description is intended to be illustrative and not limiting. Upon reading the above description, many embodiments and many applications beyond the examples provided will be apparent to those skilled in the art. Therefore, the scope of the present teachings should not be determined with reference to the above description, but should be determined with reference to the appended claims and the full scope of equivalents to which such claims are entitled. For the purpose of comprehensiveness, all articles and references, including disclosures of patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the preceding claims is not intended to be a waiver of the subject matter, nor should it be considered that the applicant has not considered the subject matter to be part of the disclosed application subject matter.

Claims

1. A method for preparing a glue-free bamboo-based filament board, characterized in that: The first state bamboo-based filaments are obtained by steam explosion treatment, wherein the length of the first state bamboo-based filaments is 6 to 10 cm and the width is 50 to 150 μm, and then the first state bamboo-based filaments are subjected to low-temperature plasma treatment to obtain the second state bamboo-based filaments, and finally the second state bamboo-based filaments are subjected to hot pressing treatment to prepare the glue-free bamboo-based filament board; The discharge power of the low-temperature plasma treatment is 300-500W, and the treatment time is 250-300s. The low-temperature plasma treatment includes the first stage to the third stage. In the first stage, the plasma treatment is carried out in a mixed gas of carbon dioxide / oxygen. In the second stage, the plasma treatment is carried out in a mixed gas of argon / helium. In the third stage, the plasma treatment is carried out in a mixed gas of ammonia / nitrogen. In the carbon dioxide / oxygen mixed gas, the ratio of carbon dioxide to oxygen is 2:8 to 8:2; in the argon / helium mixed gas, the ratio of argon to helium is 1:1; in the ammonia / nitrogen mixed gas, the ratio of ammonia to nitrogen is 1:9 to 9:

1.

2. The method for preparing the glue-free bamboo-based filament board according to claim 1, characterized in that: The low temperature plasma of the plasma treatment includes at least one of corona discharge, glow discharge, dielectric barrier discharge or radio frequency plasma.

3. The method for preparing the glue-free bamboo-based filament board according to claim 1, characterized in that: The steam explosion has a pressure of 1-4 MPa, a temperature of 120-240° C., and a pressure holding time of 30-300 seconds.

4. The method for preparing the glue-free bamboo-based filament board according to claim 1, characterized in that: Before the steam explosion treatment, the bamboo strips are pretreated; the pretreatment is that the bamboo strips are soaked in hot water at a temperature of 80 to 100° C. for 4 to 8 hours, and then soaked in cold water at room temperature for 24 to 48 hours.

5. The method for preparing the glue-free bamboo-based filament board according to claim 1, characterized in that: Before the plasma treatment, the bamboo-based filaments are ultrasonically cleaned and dispersed, and then the bamboo-based filaments are dried to a moisture content of 3 to 12%.

6. The method for preparing the glue-free bamboo-based filament board according to claim 1, characterized in that: The temperature of the hot pressing treatment is 190-250° C., the pressure is 0.5-2.5 MPa, and the time is 5-15 min to obtain the glue-free bamboo-based filament board.

Citation Information

Patent Citations

  • Method for processing wood fibers by plasma for reinforcing interface bonding capacity of fiber plate

    CN107009478A

  • Modified stalk material and its application

    CN1412092A

  • Method for the production of material plates and material plate

    AU2007276402A1

  • Method for producing glue-free fiber board by using dry method of steam explosion slurry

    CN102225571A

  • Bamboo blasting separation and self-recombination method

    CN108582337A

Cited By

  • Preparation method of bamboo shaving multilayer composite outdoor floor

    CN122275119A