A preparation process of environmentally friendly permeable concrete
By using modified resin and modified filler in permeable concrete to form hyperbranched structures and porous structures, the problem of low mechanical strength of permeable concrete is solved, and the combination of high strength and permeability is achieved, extending service life and improving The city's waterproof and heat island resistance are capable of.
Patent Information
- Application Number
- CN202410258163.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-03-07
AI Technical Summary
At this stage, the mechanical strength of permeable concrete is not high and is prone to damage, which cannot effectively solve the problems of urban waterlogging and heat island effects.
Adopt an environmentally friendly and permeable concrete preparation process, by using modified resins and modified fillers, the hyperbranched structure and porous structure are formed, the mechanical properties of concrete are improved, and the concrete is realized through dynamic covalent bonds between silicones and borates. Quick fix.
It improves the mechanical strength and water permeability of concrete, extends its service life, and can be quickly repaired after damage, effectively solving the problems of urban waterlogging and heat island effects.
Smart Images

Figure BDA0004729900780000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete preparation, and in particular to a process for preparing environmentally friendly permeable concrete. Background Art
[0002] With the development of urbanization, the area occupied by urban buildings, roads, and squares has continued to increase, meeting the needs of people's lives and work in modern society. However, a series of "urban diseases" have emerged, such as urban waterlogging, urban runoff surface pollution, and urban heat island effect. During the rainy season, many cities will experience varying degrees of waterlogging, which not only affects people's travel, but also threatens people's lives. In addition, rainwater runoff washes and carries a large amount of pollutants accumulated from roofs, community roads, municipal road surfaces, etc. during the confluence process, aggravating the pollution of rivers. The large-scale hardening of roads in towns and cities, and the large reduction in the area covered by soil and vegetation, hinder the exchange of heat and moisture in the air with the soil, and the heat absorbed by vegetation decreases, resulting in the temperature in towns being generally higher than the surrounding areas, causing an increasingly serious urban heat island effect. Therefore, high-strength permeable concrete has gradually entered people's field of vision. Summary of the invention
[0003] The purpose of the present invention is to provide an environmentally friendly permeable concrete preparation process, which solves the problem that the current permeable concrete has low mechanical strength and is easy to break.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A process for preparing environmentally friendly permeable concrete, comprising the following steps:
[0006] Weigh the following raw materials in parts by weight: 400-450 parts of cement, 150-200 parts of modified resin, 300-500 parts of modified filler, 1000-1100 parts of crushed stone aggregate, 25-30 parts of silica fume, 6-8 parts of water reducer and 130-150 parts of water, and mix the raw materials evenly to obtain environmentally friendly permeable concrete.
[0007] Further, the modified resin is prepared by the following steps:
[0008] Diaminodiphenyl disulfide, 3-glycidyl ether propyl trimethoxysilane and toluene are uniformly mixed, and reacted for 5-7 hours at a speed of 120-150 r / min, a temperature of 40-60°C and a pH value of 11-12 to obtain a modified monomer. The modified monomer, polytetrahydrofuran, diethyl 2,2-bis(hydroxymethyl)malonate, dicyclohexylmethane diisocyanate and dibutyltin dilaurate are reacted for 5-7 hours at a speed of 150-200 r / min and a temperature of 60-65°C to obtain a modified resin.
[0009] Furthermore, the molar ratio of the diaminodiphenyl disulfide to 3-glycidyl ether propyl trimethoxysilane is 1:4, the molar ratio of the modified monomer, polytetrahydrofuran, 2,2-bishydroxymethyl diethyl malonate and dicyclohexylmethane diisocyanate is 1:10:13:50, and the amount of dibutyltin dilaurate is 1-1.5% of the total mass of the modified monomer, polytetrahydrofuran and 2,2-bishydroxymethyl diethyl malonate.
[0010] Further, the modified filler is prepared by the following steps:
[0011] Step B1: dispersing basalt fiber in ethanol, adding 3-methacryloxypropyltrimethoxysilane and deionized water, reacting for 1-1.5 hours at a speed of 150-200 r / min and a temperature of 30-40° C., filtering and removing the filtrate, dispersing the substrate in DMF, adding 3-mercaptopropyltriethoxysilane and n-butyl lithium, reacting for 3-5 hours at a speed of 120-150 r / min and irradiating with 365 nm ultraviolet light, to obtain pretreated basalt fiber;
[0012] Step B2: Disperse the pretreated basalt fiber in dimethyl sulfoxide, add 3-aminopropyltriethoxysilane, react for 10-15 hours at a speed of 150-200 r / min and a temperature of 60-65° C., cool to room temperature and add ammonium fluoride, continue to react for 20-25 hours, and then age for 20-25 hours at a temperature of 80-85° C. to obtain modified basalt, mix acrylic acid, glycidol, p-toluenesulfonic acid and toluene uniformly, and reflux for 3-5 hours at a speed of 60-80 r / min and a temperature of 112-115° C. to obtain intermediate 1;
[0013] Step B3: The modified basalt fiber, intermediate 1 and dimethyl sulfoxide are mixed uniformly, and reacted for 3-5 hours at a speed of 150-200 r / min, a temperature of 50-60° C. and a pH value of 11-12 to obtain a modified matrix; the modified matrix, ethyl acrylate and sodium hydroxide solution are mixed, and stirred at a speed of 120-150 r / min and a temperature of 20-25° C., potassium persulfate and titanium dioxide sol are added, the temperature is raised to 60-65° C., and the reaction is carried out for 2-3 hours, and then added to a hydrochloric acid solution, and soaked at a temperature of 80-85° C. for 30-40 minutes to obtain a precursor;
[0014] Step B4: Mix the precursor, 4-formylphenylboronic acid and benzene evenly, reflux for 6-8 hours at a rotation speed of 120-150 r / min and a temperature of 81-83°C, filter and remove the filtrate, disperse the substrate in anhydrous ethanol, stir and add p-phenylenediamine at a rotation speed of 150-200 r / min and a temperature of 65-70°C, and react for 10-12 hours to obtain a modified filler.
[0015] Furthermore, the amount of 3-methacryloxypropyltrimethoxysilane in step B1 is 3% of the mass of basalt fiber, the molar ratio of 3-methacryloxypropyltrimethoxysilane to 3-mercaptopropyltriethoxysilane is 1:1, and the amount of n-butyl lithium is 0.3-0.5% of the mass of 3-mercaptopropyltriethoxysilane.
[0016] Furthermore, the amount ratio of the pretreated basalt fiber, 3-aminopropyltriethoxysilane and ammonium fluoride in step B2 is 2g:5mL:0.3g, the molar ratio of acrylic acid to glycidol is 1:1, and the amount ratio of p-toluenesulfonic acid is 1-1.5% of the total mass of acrylic acid and glycidol.
[0017] Furthermore, the molar ratio of the amino group on the modified basalt fiber described in step B3 to the intermediate 1 is 1:1, the dosage ratio of the modified matrix, ethyl acrylate, sodium hydroxide solution, potassium persulfate and titanium dioxide sol is 1g:5g:10mL:0.45g:10g, the concentration of the sodium hydroxide solution is 5mol / L, and the concentration of the hydrochloric acid solution is 6mol / L.
[0018] Furthermore, the amount ratio of the precursor, 4-formylphenylboronic acid and p-phenylenediamine in step B4 is 1 g: 10 mmol: 12 mmol.
[0019] Beneficial effects of the invention: An environmentally friendly permeable concrete comprises the following raw materials: cement, modified resin, modified filler, crushed stone aggregate, silica powder, water reducer and water. The modified resin uses diaminodiphenyl disulfide and 3-glycidyl ether propyl trimethoxy silane as raw materials, so that the amino group on the diaminodiphenyl disulfide reacts with the epoxy group on the 3-glycidyl ether propyl trimethoxy silane to form a new hydroxyl group, and the modified monomer, polytetrahydrofuran, 2,2-bishydroxymethyl malonate and dicyclohexylmethane diisocyanate are reacted to form an isocyanate-terminated modified resin. In the process of raw material blending, the isocyanate group on the modified resin can react with the surface of the modified filler. The modified resin is a hyperbranched structure, and the side chain contains a siloxane structure that can be hydrolyzed, and then coated with crushed stone aggregate, silica powder and cement, thereby improving the mechanical properties of concrete. The modified filler is made of basalt fiber as a raw material and treated with 3-methacryloxypropyltrimethoxysilane to graft double bonds on the surface, and then reacted with 3-mercaptopropyltriethoxysilane under ultraviolet irradiation to graft the double bonds on the surface with the mercapto groups on the 3-mercaptopropyltriethoxysilane to obtain pretreated basalt fiber. The pretreated basalt fiber is reacted with 3-aminopropyltriethoxysilane to make the siloxane groups on the surface of the pretreated basalt grafted with 3-aminopropyltriethoxysilane. The silane is hydrolyzed and condensed to form a silsesquioxane structure, acrylic acid and glycidol are reacted to esterify the carboxyl group on the acrylic acid and the hydroxyl group on the glycidol to obtain an intermediate 1, the intermediate 1 is reacted with modified basalt fiber under alkaline conditions to react the epoxy group on the intermediate 1 with the amino group on the modified basalt cellulose to obtain a modified matrix, the modified matrix and ethyl acrylate are reacted under the action of potassium persulfate to form polyacrylate on the surface, and titanium dioxide sol is embedded between the polyacrylates, and titanium dioxide is removed by treatment in a hydrochloric acid solution to form a porous structure to obtain a precursor, and the precursor is reacted with 4-formylphenylboronic acid to make 4-formylphenylboronic acid The boric acid groups on the surface of the precursor react with the hydroxyl groups on the surface of the precursor to form a borate structure, and then p-phenylenediamine is added to make the amino group on the p-phenylenediamine react with the aldehyde group to form a Schiff base structure to obtain a modified filler. The modified filler contains a large number of pores, and the modified resin will also foam when mixed with water, so that the prepared concrete has good water permeability. The modified filler is a core-shell structure, and contains a cage-type silsesquioxane support structure between the inner core and the outer shell, which can further improve the mechanical properties of the concrete. The borate structure and Schiff base structure on the modified filler are dynamic covalent bonds with the SS bonds on the modified resin, so that the concrete can be quickly repaired after damage, thereby increasing its service life. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] A process for preparing environmentally friendly permeable concrete, comprising the following steps:
[0023] The following raw materials were weighed in parts by weight: 400 parts of cement, 150 parts of modified resin, 300 parts of modified filler, 1000 parts of crushed stone aggregate, 25 parts of silica fume, 6 parts of water reducer and 130 parts of water, and the raw materials were mixed evenly to prepare environmentally friendly permeable concrete.
[0024] The water reducing agent is sodium tri(1-methylethyl)naphthalenesulfonate, the cement is P·O42.5 grade ordinary Portland cement, and the particle size of the crushed stone aggregate is 5 mm.
[0025] The modified resin is prepared by the following steps:
[0026] Diaminodiphenyl disulfide, 3-glycidyl ether propyl trimethoxysilane and toluene were mixed evenly, and reacted for 5 hours at a speed of 120 r / min, a temperature of 40°C and a pH value of 11 to obtain a modified monomer. The modified monomer, polytetrahydrofuran, diethyl 2,2-bis(hydroxymethyl)malonate, dicyclohexylmethane diisocyanate and dibutyltin dilaurate were reacted for 5 hours at a speed of 150 r / min and a temperature of 60°C to obtain a modified resin.
[0027] The molar ratio of diaminodiphenyl disulfide and 3-glycidyl ether propyl trimethoxysilane is 1:4, the molar ratio of the modified monomer, polytetrahydrofuran, 2,2-bishydroxymethyl malonate and dicyclohexylmethane diisocyanate is 1:10:13:50, the molecular weight of polytetrahydrofuran is 2000, and the amount of dibutyltin dilaurate is 1% of the total mass of the modified monomer, polytetrahydrofuran and 2,2-bishydroxymethyl malonate.
[0028] The modified filler is prepared by the following steps:
[0029] Step B1: Disperse basalt fiber in ethanol, add 3-methacryloxypropyltrimethoxysilane and deionized water, react for 1 hour at a speed of 150 r / min and a temperature of 30° C., filter and remove the filtrate, disperse the substrate in DMF, add 3-mercaptopropyltriethoxysilane and n-butyl lithium, react for 3 hours at a speed of 120 r / min and 365 nm ultraviolet light irradiation, and obtain pretreated basalt fiber;
[0030] Step B2: Disperse the pretreated basalt fiber in dimethyl sulfoxide, add 3-aminopropyltriethoxysilane, react for 10 hours at a speed of 150 r / min and a temperature of 60° C., cool to room temperature and add ammonium fluoride, continue to react for 20 hours, and then age for 20 hours at a temperature of 80° C. to obtain modified basalt, mix acrylic acid, glycidol, p-toluenesulfonic acid and toluene uniformly, and reflux for 3 hours at a speed of 60 r / min and a temperature of 112° C. to obtain intermediate 1;
[0031] Step B3: The modified basalt fiber, intermediate 1 and dimethyl sulfoxide were mixed uniformly, and reacted for 3 hours at a speed of 150 r / min, a temperature of 50°C and a pH value of 11 to obtain a modified matrix. The modified matrix, ethyl acrylate and sodium hydroxide solution were mixed, and potassium persulfate and titanium dioxide sol were added under stirring at a speed of 120 r / min and a temperature of 20°C. The mixture was heated to 60°C, reacted for 2 hours, and then added to a hydrochloric acid solution. The mixture was immersed in the solution at a temperature of 80°C for 30 minutes to obtain a precursor.
[0032] Step B4: Mix the precursor, 4-formylphenylboronic acid and benzene evenly, reflux for reaction at a speed of 120 r / min and a temperature of 81°C for 6 hours, filter and remove the filtrate, disperse the substrate in anhydrous ethanol, stir and add p-phenylenediamine at a speed of 150 r / min and a temperature of 65°C, and react for 10 hours to obtain a modified filler.
[0033] The amount of 3-methacryloxypropyltrimethoxysilane used in step B1 is 3% of the mass of basalt fiber, the molar ratio of 3-methacryloxypropyltrimethoxysilane to 3-mercaptopropyltriethoxysilane is 1:1, and the amount of n-butyl lithium used is 0.3% of the mass of 3-mercaptopropyltriethoxysilane.
[0034] The amount ratio of the pretreated basalt fiber, 3-aminopropyltriethoxysilane and ammonium fluoride described in step B2 is 2g:5mL:0.3g, the molar ratio of acrylic acid and glycidol is 1:1, and the amount ratio of p-toluenesulfonic acid is 1% of the total mass of acrylic acid and glycidol.
[0035] The molar ratio of the amino group on the modified basalt fiber and the intermediate 1 in step B3 is 1:1, the dosage ratio of the modified matrix, ethyl acrylate, sodium hydroxide solution, potassium persulfate and titanium dioxide sol is 1g:5g:10mL:0.45g:10g, the concentration of the sodium hydroxide solution is 5mol / L, and the concentration of the hydrochloric acid solution is 6mol / L.
[0036] The amount ratio of the precursor, 4-formylphenylboronic acid and p-phenylenediamine described in step B4 is 1g:10mmol:12mmol.
[0037] Example 2
[0038] A process for preparing environmentally friendly permeable concrete, comprising the following steps:
[0039] The following raw materials were weighed in parts by weight: 430 parts of cement, 180 parts of modified resin, 400 parts of modified filler, 1050 parts of crushed stone aggregate, 28 parts of silica fume, 7 parts of water reducer and 140 parts of water, and the raw materials were mixed evenly to prepare environmentally friendly permeable concrete.
[0040] The water reducing agent is sodium 6-hydroxy-2-naphthalenesulfonate, the cement is ordinary Portland cement of P·O42.5 grade, and the particle size of the crushed stone aggregate is 6 mm.
[0041] The modified resin is prepared by the following steps:
[0042] Diaminodiphenyl disulfide, 3-glycidyl ether propyl trimethoxysilane and toluene were mixed evenly, and reacted for 6 hours at a speed of 1204 r / min, a temperature of 50°C and a pH value of 12 to obtain a modified monomer. The modified monomer, polytetrahydrofuran, diethyl 2,2-bis(hydroxymethyl)malonate, dicyclohexylmethane diisocyanate and dibutyltin dilaurate were reacted for 6 hours at a speed of 150 r / min and a temperature of 63°C to obtain a modified resin.
[0043] The molar ratio of diaminodiphenyl disulfide to 3-glycidyl ether propyl trimethoxysilane is 1:4, the molar ratio of the modified monomer, polytetrahydrofuran, 2,2-bishydroxymethyl diethyl malonate and dicyclohexylmethane diisocyanate is 1:10:13:50, the molecular weight of polytetrahydrofuran is 2000, and the amount of dibutyltin dilaurate is 1.5% of the total mass of the modified monomer, polytetrahydrofuran and 2,2-bishydroxymethyl diethyl malonate.
[0044] The modified filler is prepared by the following steps:
[0045] Step B1: Disperse basalt fiber in ethanol, add 3-methacryloxypropyltrimethoxysilane and deionized water, react for 1.5 hours at a speed of 200 r / min and a temperature of 35° C., filter and remove the filtrate, disperse the substrate in DMF, add 3-mercaptopropyltriethoxysilane and n-butyl lithium, react for 4 hours at a speed of 120 r / min and 365 nm ultraviolet light irradiation, and obtain pretreated basalt fiber;
[0046] Step B2: Disperse the pretreated basalt fiber in dimethyl sulfoxide, add 3-aminopropyltriethoxysilane, react for 13 hours at a speed of 200 r / min and a temperature of 63°C, cool to room temperature and add ammonium fluoride, continue to react for 23 hours, and then age for 23 hours at a temperature of 83°C to obtain modified basalt, mix acrylic acid, glycidol, p-toluenesulfonic acid and toluene, and reflux for 4 hours at a speed of 60 r / min and a temperature of 115°C to obtain intermediate 1;
[0047] Step B3: The modified basalt fiber, intermediate 1 and dimethyl sulfoxide were mixed uniformly, and reacted for 4 hours at a speed of 150 r / min, a temperature of 55° C. and a pH value of 12 to obtain a modified matrix. The modified matrix, ethyl acrylate and sodium hydroxide solution were mixed, and potassium persulfate and titanium dioxide sol were added under stirring at a speed of 120 r / min and a temperature of 25° C. The mixture was heated to 63° C., reacted for 2.5 hours, and then added to a hydrochloric acid solution, and soaked at a temperature of 83° C. for 35 minutes to obtain a precursor.
[0048] Step B4: Mix the precursor, 4-formylphenylboronic acid and benzene evenly, reflux for reaction at a speed of 150 r / min and a temperature of 82°C for 7 hours, filter and remove the filtrate, disperse the substrate in anhydrous ethanol, stir and add p-phenylenediamine at a speed of 150 r / min and a temperature of 68°C, and react for 11 hours to obtain a modified filler.
[0049] The amount of 3-methacryloxypropyltrimethoxysilane used in step B1 is 3% of the mass of basalt fiber, the molar ratio of 3-methacryloxypropyltrimethoxysilane to 3-mercaptopropyltriethoxysilane is 1:1, and the amount of n-butyl lithium used is 0.4% of the mass of 3-mercaptopropyltriethoxysilane.
[0050] The amount ratio of the pretreated basalt fiber, 3-aminopropyltriethoxysilane and ammonium fluoride described in step B2 is 2g:5mL:0.3g, the molar ratio of acrylic acid to glycidol is 1:1, and the amount ratio of p-toluenesulfonic acid is 1.5% of the total mass of acrylic acid and glycidol.
[0051] The molar ratio of the amino group on the modified basalt fiber and the intermediate 1 in step B3 is 1:1, the dosage ratio of the modified matrix, ethyl acrylate, sodium hydroxide solution, potassium persulfate and titanium dioxide sol is 1g:5g:10mL:0.45g:10g, the concentration of the sodium hydroxide solution is 5mol / L, and the concentration of the hydrochloric acid solution is 6mol / L.
[0052] The amount ratio of the precursor, 4-formylphenylboronic acid and p-phenylenediamine described in step B4 is 1g:10mmol:12mmol.
[0053] Example 3
[0054] A process for preparing environmentally friendly permeable concrete, comprising the following steps:
[0055] The following raw materials were weighed in parts by weight: 450 parts of cement, 200 parts of modified resin, 500 parts of modified filler, 1100 parts of crushed stone aggregate, 30 parts of silica fume, 8 parts of water reducer and 150 parts of water, and the raw materials were mixed evenly to prepare environmentally friendly permeable concrete.
[0056] The water reducing agent is sodium 2,6-di-tert-butylnaphthalene sulfonate, the cement is P·O42.5 grade ordinary Portland cement, and the particle size of the crushed stone aggregate is 7 mm.
[0057] The modified resin is prepared by the following steps:
[0058] Diaminodiphenyl disulfide, 3-glycidyl ether propyl trimethoxysilane and toluene were mixed evenly, and reacted for 7 hours at a speed of 150 r / min, a temperature of 60°C and a pH value of 12 to obtain a modified monomer. The modified monomer, polytetrahydrofuran, diethyl 2,2-bis(hydroxymethyl)malonate, dicyclohexylmethane diisocyanate and dibutyltin dilaurate were reacted for 7 hours at a speed of 200 r / min and a temperature of 65°C to obtain a modified resin.
[0059] The molar ratio of diaminodiphenyl disulfide to 3-glycidyl ether propyl trimethoxysilane is 1:4, the molar ratio of the modified monomer, polytetrahydrofuran, 2,2-bishydroxymethyl diethyl malonate and dicyclohexylmethane diisocyanate is 1:10:13:50, the molecular weight of polytetrahydrofuran is 2000, and the amount of dibutyltin dilaurate is 1.5% of the total mass of the modified monomer, polytetrahydrofuran and 2,2-bishydroxymethyl diethyl malonate.
[0060] The modified filler is prepared by the following steps:
[0061] Step B1: Disperse basalt fiber in ethanol, add 3-methacryloxypropyltrimethoxysilane and deionized water, react for 1.5 hours at a speed of 200 r / min and a temperature of 40° C., filter and remove the filtrate, disperse the substrate in DMF, add 3-mercaptopropyltriethoxysilane and n-butyl lithium, react for 5 hours at a speed of 150 r / min and 365 nm ultraviolet light irradiation, and obtain pretreated basalt fiber;
[0062] Step B2: Disperse the pretreated basalt fiber in dimethyl sulfoxide, add 3-aminopropyltriethoxysilane, react for 15 hours at a speed of 200 r / min and a temperature of 65°C, cool to room temperature and add ammonium fluoride, continue to react for 25 hours, and then age for 25 hours at a temperature of 85°C to obtain modified basalt, mix acrylic acid, glycidol, p-toluenesulfonic acid and toluene, and reflux for 5 hours at a speed of 80 r / min and a temperature of 115°C to obtain intermediate 1;
[0063] Step B3: The modified basalt fiber, intermediate 1 and dimethyl sulfoxide were mixed uniformly, and reacted for 5 hours at a speed of 200 r / min, a temperature of 60°C and a pH value of 12 to obtain a modified matrix. The modified matrix, ethyl acrylate and sodium hydroxide solution were mixed, and potassium persulfate and titanium dioxide sol were added under stirring at a speed of 150 r / min and a temperature of 25°C. The temperature was raised to 65°C, and the mixture was reacted for 3 hours. The mixture was then added to a hydrochloric acid solution and soaked for 40 minutes at a temperature of 85°C to obtain a precursor.
[0064] Step B4: Mix the precursor, 4-formylphenylboronic acid and benzene evenly, reflux for reaction at a speed of 150 r / min and a temperature of 83°C for 8 hours, filter and remove the filtrate, disperse the substrate in anhydrous ethanol, stir and add p-phenylenediamine at a speed of 200 r / min and a temperature of 70°C, and react for 12 hours to obtain a modified filler.
[0065] The amount of 3-methacryloxypropyltrimethoxysilane used in step B1 is 3% of the mass of basalt fiber, the molar ratio of 3-methacryloxypropyltrimethoxysilane to 3-mercaptopropyltriethoxysilane is 1:1, and the amount of n-butyl lithium used is 0.5% of the mass of 3-mercaptopropyltriethoxysilane.
[0066] The amount ratio of the pretreated basalt fiber, 3-aminopropyltriethoxysilane and ammonium fluoride described in step B2 is 2g:5mL:0.3g, the molar ratio of acrylic acid to glycidol is 1:1, and the amount ratio of p-toluenesulfonic acid is 1.5% of the total mass of acrylic acid and glycidol.
[0067] The molar ratio of the amino group on the modified basalt fiber and the intermediate 1 in step B3 is 1:1, the dosage ratio of the modified matrix, ethyl acrylate, sodium hydroxide solution, potassium persulfate and titanium dioxide sol is 1g:5g:10mL:0.45g:10g, the concentration of the sodium hydroxide solution is 5mol / L, and the concentration of the hydrochloric acid solution is 6mol / L.
[0068] The amount ratio of the precursor, 4-formylphenylboronic acid and p-phenylenediamine described in step B4 is 1g:10mmol:12mmol.
[0069] Comparative Example 1
[0070] Compared with Example 1, this comparative example uses basalt fiber instead of modified filler, and the other steps are the same.
[0071] Comparative Example 2
[0072] Compared with Example 1, this comparative example uses modified basalt instead of modified filler, and the remaining steps are the same.
[0073] Comparative Example 3
[0074] Compared with Example 1, this comparative example uses a precursor instead of a modified filler, and the remaining steps are the same.
[0075] Comparative Example 4
[0076] Compared with Example 1, no modified resin was added in this comparative example, and the remaining steps were the same.
[0077] The concretes prepared in Examples 1-3 and Comparative Examples 1-4 were oxidized in batches for 28 days, and the compressive strength and flexural strength were tested according to the standard of GB / T50081-2002. The water permeability coefficient of the concrete cured for 28 days was measured by the constant head method. The test results are shown in the following table.
[0078]
[0079] It can be seen from the above table that the present application has good mechanical strength and water permeability.
[0080] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A process for preparing environmentally friendly permeable concrete, characterized in that: The specific steps include: Weigh the following raw materials in parts by weight: 400-450 parts of cement, 150-200 parts of modified resin, 300-500 parts of modified filler, 1000-1100 parts of crushed stone aggregate, 25-30 parts of silica fume, 6-8 parts of water reducer and 130-150 parts of water, and mix the raw materials evenly to prepare environmentally friendly permeable concrete; The modified resin is prepared by the following steps: Diaminodiphenyl disulfide, 3-glycidyl ether propyl trimethoxysilane and toluene are uniformly mixed, and reacted for 5-7 hours at a speed of 120-150 r / min, a temperature of 40-60° C. and a pH value of 11-12 to obtain a modified monomer; the modified monomer, polytetrahydrofuran, diethyl 2,2-bis(hydroxymethyl)malonate, dicyclohexylmethane diisocyanate and dibutyltin dilaurate are reacted for 5-7 hours at a speed of 150-200 r / min and a temperature of 60-65° C. to obtain a modified resin; The molar ratio of diaminodiphenyl disulfide to 3-glycidyl ether propyl trimethoxysilane is 1:4, the molar ratio of the modified monomer, polytetrahydrofuran, diethyl 2,2-bishydroxymethyl malonate and dicyclohexylmethane diisocyanate is 1:10:13:50, and the amount of dibutyltin dilaurate is 1-1.5% of the total mass of the modified monomer, polytetrahydrofuran and diethyl 2,2-bishydroxymethyl malonate; The modified filler is prepared by the following steps: Step B1: dispersing basalt fiber in ethanol, adding 3-methacryloxypropyltrimethoxysilane and deionized water, reacting for 1-1.5 hours at a speed of 150-200 r / min and a temperature of 30-40° C., filtering and removing the filtrate, dispersing the substrate in DMF, adding 3-mercaptopropyltriethoxysilane and n-butyl lithium, reacting for 3-5 hours at a speed of 120-150 r / min and irradiating with 365 nm ultraviolet light, to obtain pretreated basalt fiber; Step B2: Disperse the pretreated basalt fiber in dimethyl sulfoxide, add 3-aminopropyltriethoxysilane, react for 10-15 hours at a speed of 150-200 r / min and a temperature of 60-65° C., cool to room temperature and add ammonium fluoride, continue to react for 20-25 hours, and then age for 20-25 hours at a temperature of 80-85° C. to obtain modified basalt, mix acrylic acid, glycidol, p-toluenesulfonic acid and toluene uniformly, and reflux for 3-5 hours at a speed of 60-80 r / min and a temperature of 112-115° C. to obtain intermediate 1; Step B3: The modified basalt fiber, intermediate 1 and dimethyl sulfoxide are mixed uniformly, and reacted for 3-5 hours at a speed of 150-200 r / min, a temperature of 50-60° C. and a pH value of 11-12 to obtain a modified matrix; the modified matrix, ethyl acrylate and sodium hydroxide solution are mixed, and stirred at a speed of 120-150 r / min and a temperature of 20-25° C., potassium persulfate and titanium dioxide sol are added, the temperature is raised to 60-65° C., and the reaction is carried out for 2-3 hours, and then added to a hydrochloric acid solution, and soaked at a temperature of 80-85° C. for 30-40 minutes to obtain a precursor; Step B4: Mix the precursor, 4-formylphenylboronic acid and benzene evenly, reflux for 6-8 hours at a rotation speed of 120-150 r / min and a temperature of 81-83°C, filter and remove the filtrate, disperse the substrate in anhydrous ethanol, stir and add p-phenylenediamine at a rotation speed of 150-200 r / min and a temperature of 65-70°C, and react for 10-12 hours to obtain a modified filler.
2. The process for preparing an environmentally friendly permeable concrete according to claim 1, characterized in that: The amount of 3-methacryloxypropyltrimethoxysilane used in step B1 is 3% of the mass of basalt fiber, and the molar ratio of 3-methacryloxypropyltrimethoxysilane to 3-mercaptopropyltriethoxysilane is 1:
1.
3. The process for preparing an environmentally friendly permeable concrete according to claim 1, characterized in that: The amount ratio of the pretreated basalt fiber, 3-aminopropyltriethoxysilane and ammonium fluoride in step B2 is 2g:5mL:0.3g, and the molar ratio of acrylic acid to glycidol is 1:
1.
4. The process for preparing an environmentally friendly permeable concrete according to claim 1, characterized in that: The molar ratio of the amino group on the modified basalt fiber and the intermediate 1 in step B3 is 1:1, and the amount ratio of the modified matrix, ethyl acrylate, sodium hydroxide solution, potassium persulfate and titanium dioxide sol is 1g:5g:10mL:0.45g:10g.
5. The process for preparing an environmentally friendly permeable concrete according to claim 1, characterized in that: The amount ratio of the precursor, 4-formylphenylboronic acid and p-phenylenediamine in step B4 is 1 g: 10 mmol: 12 mmol.
Citation Information
Cited By
Method for rapidly repairing road surface
US12503819B2
Method for rapidly repairing road surface
US20230045473A1