Anti-PID EVA film for photovoltaic encapsulation materials
By using materials such as nano-alkaline metal oxides and crown ethers to prepare acid scavengers in photovoltaic packaging materials, the problem of free acetic acid and PID caused by the aging of EVA film in extreme weather is solved, achieving efficient acid removal and resistance to PID. performance, extending the service life of photovoltaic modules.
Patent Information
- Application Number
- CN202410299842.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-15
AI Technical Summary
The photovoltaic encapsulation material EVA film ages in extreme weather, leading to the generation of free acetic acid and potential induced decay (PID). The dispersion problem of inorganic alkaline fillers in the existing technology and the poor acid removal effect affect the use of photovoltaic modules. life.
Using nano-alkaline metal oxides, silane coupling agents, crown ethers and other materials for blending reactions, an acid scavenger is prepared through the neutralization reaction of alkaline metal oxides and free acetic acid and the reaction of crown ethers on metal cations. The complexing effect improves the acid removal and PID resistance performance of the film.
It achieves excellent acetic acid adsorption and PID resistance, while maintaining the mechanical properties and light transmittance of the film, extending the service life of photovoltaic modules.
Smart Images

Figure CN118126648B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an anti-PID EVA film for photovoltaic packaging materials and belongs to the field of photovoltaic materials. Background Art
[0002] As a part of solar cells, EVA (ethylene-vinyl acetate copolymer) film is used outdoors for a long time and encounters extreme weather. Thermal, light and oxygen aging always accompanies the EVA film. The aging of EVA film begins with the decomposition of its molecular chain, releasing small molecules of acetic acid. The presence of free acetic acid will form a weakly acidic environment, which will catalyze further decomposition. The whole process is an "automatic acceleration" phenomenon.
[0003] At present, most of the existing technologies use inorganic alkaline fillers to neutralize free acetic acid, but there are also problems with the dispersibility of inorganic fillers, and the acid removal effect is not good; as well as a series of problems such as mechanical properties, light transmittance, and aging resistance.
[0004] In addition, another issue that affects the service life of photovoltaic modules is the potential induced degradation (PID) effect of photovoltaic modules. The PID effect can lead to catastrophic failure. The main reasons for the PID effect include the following: (1) installation method; (2) climatic conditions at the site of use; (3) type of photovoltaic module cells; (4) materials used in photovoltaic modules: photovoltaic modules contain glass, encapsulation film, cells and backplanes. In actual applications, the module materials induce Na+ migration to varying degrees, thereby causing the PID effect. From the perspective of materials, the study of anti-PID effect is currently mainly aimed at the mechanism of Na+ migration inducing PID effect of crystalline silicon modules, reducing the internal ion mobility of EVA encapsulation film to prevent the PID effect caused by Na+ migration.
[0005] In addition, the biggest feature of crown ethers is that they can form stable complexes with guest molecules such as metal ions and ammonium ions as hosts, such as crown ethers and all ions of the first and second main groups in the periodic table, cadmium, mercury, lead in transition elements, and lanthanide and actinide ions.
[0006] Considering the problem of free acid generated by EVA film and the practical problem of inorganic alkaline fillers, the dispersibility of inorganic alkaline fillers can be improved through chemical modification. Combined with the characteristics of crown ether as a metal ion scavenger, it is of great practical significance to make a self-made EVA acid scavenger and anti-PID EVA film for photovoltaic packaging materials through chemical modification. Summary of the invention
[0007] The purpose of the present invention is to solve the problem that the photovoltaic encapsulation EVA film in the prior art is used for a long time in an outdoor environment, and is aged by light, heat, and oxygen to produce free acetic acid and cause PID. In combination with the neutralization of free acetic acid by alkaline metal oxides and the complexation of metal cations by crown ether structures, an anti-PID EVA film for photovoltaic encapsulation materials and a preparation method thereof are provided. The film has excellent acetic acid adsorption and anti-PID, and also has excellent mechanical properties. The technical solution adopted by the present invention to solve the technical problem is:
[0008] A method for preparing an acid scavenger comprises the following steps:
[0009] Step S11, placing the nano-alkaline metal oxide and the silane coupling agent in an alcohol solvent to carry out a silanization coupling reaction to obtain a silane-modified metal oxide;
[0010] Step S12, copolymerizing the olefin derivative and choline containing a carbon-carbon double bond under the action of a thermal initiator to obtain a polymer containing a choline structure; and
[0011] Step S13, blending the silane-modified metal oxide, the polymer containing the choline structure, and the crown ether to obtain the target product, namely, the acid scavenger.
[0012] Furthermore, the silane coupling agent is an aminosilane coupling agent; and
[0013] The dosage ratio of the nanometer basic metal oxide, the silane coupling agent and the alcohol solvent is 1g:3.5-5.5g:80mL.
[0014] Furthermore, the olefin derivative is an epoxyolefin or an aminoolefin; and
[0015] The choline containing a carbon-carbon double bond is a choline structure containing a carbon-carbon double bond and a phosphate.
[0016] Further,
[0017] The usage ratio of the olefin derivative and the choline containing a carbon-carbon double bond is 3.0-5.0 mol: 5.0-7.0 mol; and
[0018] The amount of the thermal initiator used is 1.0-1.5% of the total mass of the reactants.
[0019] Furthermore, the crown ether is 15-crown-5.
[0020] Further,
[0021] The usage ratio of the silane-modified metal oxide, the polymer containing a choline structure and the crown ether is 4.5-6.5g: 5.0-5.5g: 4.0-4.0g.
[0022] The invention also provides an acid scavenger prepared by the preparation method.
[0023] The present invention also provides an anti-PID EVA film for photovoltaic encapsulation materials, comprising the following raw materials in parts by weight:
[0024] EVA resin 100 parts;
[0025] Cross-linking agent 0.8-1.3 parts;
[0026] 1.2-1.8 parts of auxiliary cross-linking agent;
[0027] 2.5-4.5 parts of acid scavenger;
[0028] Antioxidant 0.1-0.3 parts;
[0029] Light stabilizer 0.1-0.2 parts;
[0030] Coupling agent 0.3-0.5 parts.
[0031] Furthermore, the cross-linking agent is an organic peroxide cross-linking agent.
[0032] Furthermore, the auxiliary cross-linking agent is allyl and / or acryloxy.
[0033] The present invention also provides a method for preparing an anti-PID EVA film for photovoltaic encapsulation materials, comprising the following steps:
[0034] S21, mixing, i.e.
[0035] Adding raw materials into a mixer according to the formula ratio, mixing and stirring to obtain mixed raw materials;
[0036] S22, extrusion, i.e.
[0037] placing the mixed raw materials in S21 in an extruder for melt blending, extrusion, casting, and cooling; and
[0038] S23, film formation, i.e.
[0039] After thickness measurement, edge pressing, shaping, edge trimming and rolling, the PID-resistant EVA film for photovoltaic encapsulation material is obtained.
[0040] Beneficial effects of the present invention:
[0041] (1) The present invention provides an anti-PID EVA film for photovoltaic encapsulation materials, wherein the formula system contains a self-made acid scavenger, including nano metal oxides, silane, amino groups, crown ethers, ammonium salts, phosphates and other structures. First, the nano metal oxides are nano-sized and will not have a negative impact on the optical properties of the EVA film; at the same time, after being modified by silane, they have excellent dispersibility; second, the alkaline metal oxides can react with free acetic acid to react with acid and base to quickly remove the free acid structure; and the nano structure has a large specific surface area and has a rapid response to free acetic acid; third, the amino structure in the acid scavenger is alkaline and can be neutralized with free acetic acid to form salts to reduce the content of free acetic acid in the system; fourth, the crown ether has an excellent complexing effect on metal cations, especially alkali metal ions, and has an anti-PID effect; fifth, the phosphate structure can effectively capture sodium ions, further improving the anti-PID performance; sixth, after the crown ether complexes with metal cations, the adsorption capacity of anions is enhanced, which is conducive to the adsorption of phosphates and acetic acid, further improving the acid binding performance, and having a synergistic acid removal and anti-PID effect.
[0042] (2) The present invention provides an anti-PID EVA film for photovoltaic encapsulation materials. The crosslinking agent in the formula system is designed by using a crosslinking agent and an auxiliary crosslinking agent to improve the crosslinking density of the EVA film, which has a positive effect on limiting the diffusion of free acetic acid and metal ions (mainly sodium ions), slowing down the aggregation of ions on the surface of EVA and glass to the surface of the battery, and reducing the aging rate.
[0043] (3) The present invention provides a method for preparing an anti-PID EVA film for photovoltaic packaging materials. The acid scavenger in the formula system uses nano-metal oxides, alkaloids, crown ethers and other raw materials as raw materials, which have a wide range of sources and are green and environmentally friendly. It is highly operational and has practical significance for the industrialization of the product of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a comparison chart of free acetic acid inventory / PID power attenuation of Example 1 and Comparative Examples 1-13. DETAILED DESCRIPTION
[0045] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0046] The purpose of the present invention is to develop an EVA encapsulation film with acid removal and anti-PID functions to meet its use in the photovoltaic field under extreme weather. The idea of realization is: to make a self-made auxiliary agent that has both the function of absorbing free acetic acid and anti-PID, and to ensure its compatibility and dispersibility in EVA. Specifically: alkaline metal oxides and the like have excellent acid-base neutralization effects on free acetic acid, and their dispersibility problems can be solved after organic chain modification; combined with the adsorption of crown ethers, phosphates and the like to sodium ions, auxiliary agents with acid removal and anti-PID functions can be prepared. The theoretical basis for realization is: after using aminosilane to modify alkaline metal oxides, the complexation of amino groups and crown ethers is utilized to form alkaline metal oxides wrapped by crown ethers, and the complexation of amino groups (ammonium salts) and crown ethers is also utilized to add a phosphorus-containing choline structure for the outermost layer of wrapping, which is an organic structure wrapping inorganic matter, and has excellent dispersibility. So far, the preparation of the acid scavenger has been completed. The basic metal oxide, amino (and epoxy) and other structures in the structure have excellent free acetic acid adsorption, and the crown ether, phosphate (and the hydroxyl structure formed after the epoxy ring opening) have excellent capture ability for sodium ions; and the cations formed after the sodium ions are captured by the crown ether have enhanced adsorption capacity for anions such as phosphate and acetate, which can further improve the acid removal and anti-PID performance. The embodiments of the present invention are as follows:
[0047] The present invention provides a method for preparing an acid scavenger, comprising the following steps:
[0048] Step S11, adding nanometer alkaline metal oxide and silane coupling agent to an alcohol solvent, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50-80° C. for 2-10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified metal oxide;
[0049] The dosage ratio of the nano alkaline metal oxide, the silane coupling agent and the alcohol solvent is 1g: 3.5-5.5g: 80mL;
[0050] The nanometer basic metal oxide in the present invention can be nanometer magnesium oxide, nanometer zinc oxide or nanometer aluminum oxide;
[0051] The nano magnesium oxide, model VK-Mg30, was purchased from Xuancheng Jingrui New Materials Co., Ltd.
[0052] The nano zinc oxide, model VK-J50H, was purchased from Xuancheng Jingrui New Materials Co., Ltd.; and
[0053] The nano alumina, model VK-L30, was purchased from Xuancheng Jingrui New Materials Co., Ltd.
[0054] The silane coupling agent in the present invention is an aminosilane coupling agent, which can be KH901, KH902, KH540, KH550, KH602, KH792; and KH550 is preferred;
[0055] The alcohol solvent in the present invention can be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.
[0056] Step S12, adding olefin derivatives, choline containing carbon-carbon double bonds, and thermal initiator AIBN to 1,4-dioxane, heating to 75-85° C., and stirring for 6-10 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60° C. for 6 hours to obtain a polymer containing a choline structure;
[0057] The usage ratio of the olefin derivative and the choline containing a carbon-carbon double bond is 3.0-5.0 mol: 5.0-7.0 mol; and
[0058] The amount of the thermal initiator AIBN is 1.0-1.5% of the total mass of the reactants;
[0059] The olefin derivatives described in the present invention are epoxyolefins or aminoolefins; the olefin derivatives can be copolymerized with choline containing a carbon-carbon double bond, and the epoxy group or amino group can adsorb free acetic acid, thereby improving the acid removal efficiency of the acid scavenger;
[0060] The epoxy olefins may be glycidyl methacrylate and / or allyl glycidyl ether; the hydroxyl structure formed by the ring-opening reaction between the epoxy group and the amino group or free acetic acid has a good capture effect on sodium ions, and the capture mechanism is as follows:
[0061] R-OH+Na + →R-ONa+H +
[0062] By capturing free sodium ions, the PID phenomenon of EVA film can be effectively reduced;
[0063] The aminoolefin may be acrylamide.
[0064] The choline containing a carbon-carbon double bond in the present invention is a choline structure containing a carbon-carbon double bond and a phosphate, which is a zwitterionic structure, and the ammonium ion can be complexed with the crown ether to form a complex; the phosphate eradication has a good complexing effect on transition metals and rare earth metals, and also has an excellent capture effect on sodium ions, which can effectively reduce the PID phenomenon of the EVA film. The choline containing a carbon-carbon double bond is a choline structure containing a carbon-carbon double bond and a phosphate, which can be soybean lecithin, 2-methacryloyloxyethyl phosphorylcholine or phosphorylcholine, etc.; and soybean lecithin is preferred.
[0065] Step S13, adding the polymer containing a choline structure into acetone, stirring and fully dissolving; adding the silane-modified metal oxide and the crown ether into the methanol solvent, ultrasonically dispersing for 0.5 hours, and standing; dropping the acetone solution of the polymer containing a choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0066] The usage ratio of the silane-modified metal oxide, the polymer containing a choline structure, and the crown ether is 4.5-6.5 g: 5.0-5.5 g: 4.0-5.0 g;
[0067] The crown ether described in the present invention is 15-crown-5; the biggest feature of crown ether is that it can form stable complexes with guest molecules such as metal ions and ammonium ions as a host. It forms complexes with positive ions, especially alkali metal ions, and coordinates with different metal ions depending on the size of the ring; the pores of 15-crown-5 can complex sodium ions or smaller lithium ions, but cannot complex larger potassium ions; at the same time, the complexing efficiency for smaller lithium ions is lower; similarly, crown ethers with smaller pores or crown ethers with larger pores cannot complex sodium ions or the complexing efficiency is low. 15-crown-5 is selected in the following embodiments of the present invention.
[0068] Silane-modified metal oxides and crown ethers are first added to the reaction system, and the complexation (electrostatic force and hydrogen bond force) between amino groups and crown ethers is used to form a structure with the crown ether wrapped in the outer layer; then a polymer containing a choline structure is added, and the ammonium ions in the choline are complexed with the crown ether to form a coordination structure. At the same time, the alkyl chain in the choline structure also forms a dipole-dipole effect with the crown ether, thereby improving the stability of the complex.
[0069] In the present invention, the acid scavenger uses an alkaline metal oxide as the core of the acid scavenger and a crown ether as the intermediate complexing layer. In the actual application process, sodium ions migrate and are captured by the crown ether. Since the ion size of the sodium ions matches the molecular pores of 15-crown ether-5, it is easier to form a complex, and the ammonium ions are replaced in the form of ion exchange to form a sodium ion complex of 15-crown ether-5. Its adsorption capacity for anions is enhanced, and it has a stronger adsorption capacity for acetate and phosphate. On the one hand, there are a large number of alkaline metal oxides, amino groups (and epoxy groups) and other groups that can adsorb acetic acid structures in the local environment of 15-crown ether-5; on the other hand, it cooperates with phosphate groups (a large number of hydroxyl structures are formed after the epoxy group reacts) to capture sodium ions, thereby improving the overall acid removal efficiency and anti-PID performance.
[0070] The present invention also provides an anti-PID EVA film for photovoltaic encapsulation materials, comprising the following raw materials in parts by weight:
[0071] EVA resin 100 parts;
[0072] Cross-linking agent 0.8-1.3 parts;
[0073] 1.2-1.8 parts of auxiliary cross-linking agent;
[0074] 2.5-4.5 parts of acid scavenger;
[0075] Antioxidant 0.1-0.3 parts;
[0076] Light stabilizer 0.1-0.2 parts;
[0077] Coupling agent 0.3-0.5 parts.
[0078] The EVA resin described in the present invention has a VA content of 28-33%. In the present embodiment, the EVA resin with a VA content of 33% and a melt index (MI) of 31 is preferably purchased from DuPont Company of the United States.
[0079] The crosslinking agent described in the present invention is an organic peroxide; it can be benzoyl peroxide, 2,5-dimethyl-2,5-bis(benzoyl peroxide)hexane, dicyclohexyl peroxycarbonate or diisopropylbenzene peroxide, etc.; the crosslinking agent described in the following embodiments of the present invention is 2,5-dimethyl-2,5-bis(benzoyl peroxide)hexane.
[0080] The auxiliary cross-linking agent in the present invention is allyl and / or acryloxy.
[0081] The allyl cross-linking auxiliary agent may be triallyl cyanurate or triallyl isocyanurate.
[0082] The acryloxy-based co-crosslinking agent may be any combination of trimethylolpropane trimethacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, propoxylated neopentyl glycol diacrylate, and pentaerythritol triacrylate.
[0083] The auxiliary cross-linking agent described in the following embodiments of the present invention is triallyl isocyanurate, trimethylolpropane trimethacrylate, propoxylated trimethylolpropane triacrylate and pentaerythritol triacrylate added in a mass ratio of 6:3:4:2.
[0084] The antioxidant described in the present invention is a combination of hindered phenols and phosphites. The hindered phenol antioxidant can be antioxidant 1010, antioxidant 1076, antioxidant 264 or antioxidant 2246, etc.; and antioxidant 1010 is preferred. The phosphite antioxidant can be antioxidant 168, antioxidant 242 or antioxidant TPP, etc.; and antioxidant 168 is preferred. In the following embodiments of the present invention, the antioxidant is antioxidant 1010 and antioxidant 168 added in a mass ratio of 1:2.
[0085] The light stabilizer described in the present invention is a combination of hindered amines and benzophenones. The hindered amines may be UV-292, UV-770 or GW540, etc., and UV-292 is preferred. The benzophenone light stabilizer may be UV-0, UV-9, UV-24 or UV-531, etc., and UV-531 is preferred. In the following embodiments of the present invention, the light stabilizers are UV-292 and UV-531 added in a mass ratio of 1:2.
[0086] The coupling agent described in the following embodiments of the present invention is a silane coupling agent, specifically a vinyl silane coupling agent, which may be KH151 or KH171, etc., and KH171 is preferred.
[0087] In order to better understand the above invention, a method for preparing an anti-PID EVA film for photovoltaic encapsulation material in the following embodiment of the present invention comprises the following steps:
[0088] S21, mixing, i.e.
[0089] Add the raw materials according to the formula ratio into a mixer, mix and stir at a temperature of 40° C. and a rotation speed of 80 rpm for 2 h to obtain a mixed raw material;
[0090] S22, extrusion, i.e.
[0091] The mixed raw materials in S21 are placed in a twin-screw extruder, melt-blended and extruded at a speed of 50 rpm with the temperature of the first zone being 80° C., the temperature of the second zone being 90° C., and the temperature of the third zone being 85° C., and the material is discharged through a cast film die head and cast, and cooled by a cast roller;
[0092] S23, film formation, i.e.
[0093] After thickness measurement, edge pressing, shaping, edge trimming and rolling, the anti-oxidation battery encapsulation EVA film with a thickness of 500 μm is obtained.
[0094] In order to further understand the present invention, an anti-PID EVA film for photovoltaic encapsulation material provided by the present invention is described in detail below in conjunction with specific embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0095] Example 1
[0096] A method for preparing an acid scavenger comprises the following steps:
[0097] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0098] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0099] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0100] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0101] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0102] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0103] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0104] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0105] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0106] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3+ (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0107] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0108] EVA resin 100 parts;
[0109] 1.0 part of cross-linking agent;
[0110] 1.5 parts of auxiliary cross-linking agent;
[0111] 3.5 parts of acid scavenger;
[0112] 0.2 parts of antioxidant;
[0113] Light stabilizer 0.15 parts;
[0114] Coupling agent KH171 0.4 parts.
[0115] Example 2
[0116] A method for preparing an acid scavenger comprises the following steps:
[0117] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0118] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550, and anhydrous ethanol is 1g:3.5g:80mL;
[0119] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0120] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0121] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0122] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0123] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0124] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0125] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0126] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm-1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0127] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0128] Example 3
[0129] A method for preparing an acid scavenger comprises the following steps:
[0130] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0131] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550, and anhydrous ethanol is 1g:5.5g:80mL;
[0132] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0133] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0134] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0135] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0136] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0137] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0138] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0139] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0140] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0141] Example 4
[0142] A method for preparing an acid scavenger comprises the following steps:
[0143] Step S11, adding nano-alumina and silane coupling agent KH550 to anhydrous ethanol, ultrasonically vibrating for 0.5 h, standing at room temperature for 2 h, reacting at 50° C. for 10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified alumina;
[0144] The dosage ratio of the nano-alumina, silane coupling agent KH550, and anhydrous ethanol is 1g:4.5g:80mL;
[0145] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm-1 、801cm -1 :-Si-O- exists; 610cm -1 、771cm -1 :Al-O exists.
[0146] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0147] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0148] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0149] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0150] Step S13, adding the polymer containing a choline structure into acetone, stirring and fully dissolving; adding silane-modified alumina and 15-crown ether-5 into a methanol solvent, ultrasonically dispersing for 0.5 hours, and standing; dropping the acetone solution of the polymer containing a choline structure into the methanol system, ultrasonically dispersing it uniformly, and volatilizing it naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0151] The usage ratio of the silane-modified alumina, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0152] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1:-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 610cm -1 、771cm -1 :Al-O exists.
[0153] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0154] Example 5
[0155] A method for preparing an acid scavenger comprises the following steps:
[0156] Step S11, adding nano zinc oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 80° C. for 2 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified zinc oxide;
[0157] The dosage ratio of the nano zinc oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0158] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 536cm -1 : Zn-O exists.
[0159] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0160] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0161] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0162] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm-1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0163] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified zinc oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0164] The usage ratio of the silane-modified zinc oxide, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0165] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 536cm -1 : Zn-O exists.
[0166] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0167] Example 6
[0168] A method for preparing an acid scavenger comprises the following steps:
[0169] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0170] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0171] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0172] Step S12, adding allyl glycidyl ether, glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 85°C, and stirring for 6 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0173] The usage ratio of allyl glycidyl ether, glycidyl methacrylate and soybean lecithin is 3.0 mol: 2.0 mol: 5.0 mol;
[0174] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0175] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0176] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0177] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0178] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1: -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0179] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0180] Example 7
[0181] A method for preparing an acid scavenger comprises the following steps:
[0182] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0183] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0184] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0185] Step S12, adding acrylamide, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 75°C, and stirring for 10 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0186] The usage ratio of acrylamide and soybean lecithin is 3.0 mol:7.0 mol;
[0187] The amount of the thermal initiator AIBN is 1.5% of the total mass of the reactants;
[0188] Its infrared data are as follows: 1670-1735cm -1 :-C=O exists; 3205cm -1 :-NH2 exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0189] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0190] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 5.5 g: 5.2 g: 4.4 g;
[0191] Its infrared data is as follows: 3426cm -1 :-OH exists; 3189cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1670-1735cm -1 :-C=O exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0192] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0193] Example 8
[0194] A method for preparing an acid scavenger comprises the following steps:
[0195] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0196] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0197] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0198] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0199] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0200] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0201] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0202] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0203] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 4.5 g: 5.0 g: 4.0 g;
[0204] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0205] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0206] Example 9
[0207] A method for preparing an acid scavenger comprises the following steps:
[0208] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0209] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0210] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0211] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80°C, and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60°C for 6 hours to obtain a polymer containing a choline structure
[0212] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0213] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0214] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0215] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0216] The usage ratio of the silane-modified magnesium oxide, the polymer containing a choline structure, and 15-crown ether-5 is 6.5 g: 5.5 g: 5.0 g;
[0217] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0218] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0219] Example 10
[0220] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0221] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0222] EVA resin 100 parts;
[0223] 1.0 part of cross-linking agent;
[0224] 1.5 parts of auxiliary cross-linking agent;
[0225] 2.5 parts of acid scavenger;
[0226] 0.2 parts of antioxidant;
[0227] Light stabilizer 0.15 parts;
[0228] Coupling agent KH171 0.4 parts.
[0229] Embodiment 11
[0230] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0231] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0232] EVA resin 100 parts;
[0233] 1.0 part of cross-linking agent;
[0234] 1.5 parts of auxiliary cross-linking agent;
[0235] 4.5 parts of acid scavenger;
[0236] 0.2 parts of antioxidant;
[0237] Light stabilizer 0.15 parts;
[0238] Coupling agent KH171 0.4 parts.
[0239] Example 12
[0240] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0241] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0242] EVA resin 100 parts;
[0243] 0.8 part of cross-linking agent;
[0244] 1.8 parts of auxiliary cross-linking agent;
[0245] 3.5 parts of acid scavenger;
[0246] 0.2 parts of antioxidant;
[0247] Light stabilizer 0.15 parts;
[0248] Coupling agent KH171 0.4 parts.
[0249] Example 13
[0250] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0251] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0252] EVA resin 100 parts;
[0253] 1.3 parts of cross-linking agent;
[0254] 1.2 parts of auxiliary cross-linking agent;
[0255] 3.5 parts of acid scavenger;
[0256] 0.2 parts of antioxidant;
[0257] Light stabilizer 0.15 parts;
[0258] Coupling agent KH171 0.4 parts.
[0259] Embodiment 14
[0260] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0261] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0262] EVA resin 100 parts;
[0263] 1.0 part of cross-linking agent;
[0264] 1.5 parts of auxiliary cross-linking agent;
[0265] 3.5 parts of acid scavenger;
[0266] Antioxidant 0.1 part;
[0267] Light stabilizer 0.2 parts;
[0268] Coupling agent KH171 0.4 parts.
[0269] Embodiment 15
[0270] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0271] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0272] EVA resin 100 parts;
[0273] 1.0 part of cross-linking agent;
[0274] 1.5 parts of auxiliary cross-linking agent;
[0275] 3.5 parts of acid scavenger;
[0276] 0.3 parts of antioxidant;
[0277] Light stabilizer 0.1 part;
[0278] Coupling agent KH171 0.4 parts.
[0279] Example 16
[0280] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0281] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0282] EVA resin 100 parts;
[0283] 1.0 part of cross-linking agent;
[0284] 1.5 parts of auxiliary cross-linking agent;
[0285] 3.5 parts of acid scavenger;
[0286] 0.2 parts of antioxidant;
[0287] Light stabilizer 0.15 parts;
[0288] Coupling agent KH171 0.3 parts.
[0289] Embodiment 17
[0290] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0291] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0292] EVA resin 100 parts;
[0293] 1.0 part of cross-linking agent;
[0294] 1.5 parts of auxiliary cross-linking agent;
[0295] 3.5 parts of acid scavenger;
[0296] 0.2 parts of antioxidant;
[0297] Light stabilizer 0.15 parts;
[0298] Coupling agent KH171 0.5 parts.
[0299] The PID-resistant EVA films for photovoltaic encapsulation materials of Comparative Examples 1-13 were compared with Example 1:
[0300] Comparative Example 1
[0301] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0302] EVA resin 100 parts;
[0303] 1.0 part of cross-linking agent;
[0304] 1.5 parts of auxiliary cross-linking agent;
[0305] 0.2 parts of antioxidant;
[0306] Light stabilizer 0.15 parts;
[0307] Coupling agent KH171 0.4 parts.
[0308] Comparative Example 2
[0309] A method for preparing an acid scavenger comprises the following steps:
[0310] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0311] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0312] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0313] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0314] Comparative Example 3
[0315] A method for preparing an acid scavenger comprises the following steps:
[0316] Step S11, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80° C., and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60° C. for 6 hours to obtain a polymer containing a choline structure;
[0317] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0318] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0319] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0320] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0321] Comparative Example 4
[0322] A method for preparing an acid scavenger comprises the following steps:
[0323] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0324] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0325] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0326] Step S12, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80° C., and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60° C. for 6 hours to obtain a polymer containing a choline structure;
[0327] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0328] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0329] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0330] Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified magnesium oxide into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0331] The usage ratio of the silane-modified magnesium oxide and the polymer containing the choline structure is 5.5 g:5.2 g;
[0332] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 peak exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0333] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0334] Comparative Example 5
[0335] A method for preparing an acid scavenger comprises the following steps:
[0336] Step S11, adding nano magnesium oxide and silane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 6 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain silane-modified magnesium oxide;
[0337] The dosage ratio of the nano magnesium oxide, silane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL;
[0338] Its infrared data is as follows: 3438cm -1 :-OH weakened; 3312cm -1 :-NH2 sharp peak exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0339] Step S12, adding silane-modified magnesium oxide and 15-crown ether-5 into methanol solvent, ultrasonically dispersing for 0.5 h, standing, and naturally volatilizing at room temperature to obtain the target product, i.e., the acid scavenger;
[0340] The usage ratio of the silane-modified magnesium oxide and 15-crown ether-5 is 5.5 g:4.4 g;
[0341] Its infrared data is as follows: 3426cm -1 :-OH exists; 3201cm -1 : -NH2 (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy groups exist; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists; 1109cm -1 、801cm -1 :-Si-O- exists; 592cm -1 : Mg-O exists.
[0342] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0343] Comparative Example 6
[0344] A method for preparing an acid scavenger comprises the following steps:
[0345] Step S11, adding glycidyl methacrylate, soybean lecithin, and thermal initiator AIBN to 1,4-dioxane, heating to 80° C., and stirring for 8 hours; after the reaction is completed, cooling to room temperature, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 60° C. for 6 hours to obtain a polymer containing a choline structure;
[0346] The usage ratio of glycidyl methacrylate and soybean lecithin is 4.0 mol:6.0 mol;
[0347] The amount of the thermal initiator AIBN is 1.0% of the total mass of the reactants;
[0348] Its infrared data are as follows: 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1622cm -1 、1603cm -1 、810cm -1 :-C=C- does not exist.
[0349] Step S12, adding the polymer containing the choline structure into acetone, stirring and fully dissolving; adding 15-crown ether-5, ultrasonically dispersing for 0.5h, and standing; volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger;
[0350] The usage ratio of the polymer containing choline structure and 15-crown ether-5 is 5.2g:4.4g;
[0351] Its infrared data are as follows: 3136cm -1 :-NH3 + (combined with O) exists; 1735cm -1 :-C=O exists; 1220cm -1 、1105cm -1 : Epoxy group exists; 1187cm -1 :-P=O exists; 1160cm -1 、978cm -1 、853cm -1 : Crown ether -COC- exists.
[0352] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0353] Comparative Example 7
[0354] The preparation method of an acid scavenger is the same as that of specific embodiment 1, except that soybean lecithin is replaced by methyl methacrylate.
[0355] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0356] Comparative Example 8
[0357] The preparation method of an acid scavenger is the same as that of specific embodiment 1, except that glycidyl methacrylate is replaced by methyl methacrylate.
[0358] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0359] Comparative Example 9
[0360] The preparation method of an acid scavenger is the same as that of specific embodiment 1, except that 15-crown-5 is replaced by 12-crown-4.
[0361] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0362] Comparative Example 10
[0363] The preparation method of an acid scavenger is the same as that of specific embodiment 1, except that 15-crown-5 is replaced by 18-crown-6.
[0364] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0365] Comparative Example 11
[0366] A method for preparing an acid scavenger comprises the following steps: blending silane-modified magnesium oxide, a polymer containing a choline structure, and 15-crown ether-5 in a mass ratio of 5.5 g:5.2 g:4.4 g to obtain the acid scavenger.
[0367] The preparation method of the silane-modified magnesium oxide is the same as that in Specific Example 1.
[0368] The preparation method of the polymer containing choline structure is the same as that of specific embodiment 1.
[0369] A PID-resistant EVA film for photovoltaic encapsulation material, the raw material components of which are the same as those in specific embodiment 1.
[0370] Comparative Example 12
[0371] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0372] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0373] EVA resin 100 parts;
[0374] 1.5 parts of auxiliary cross-linking agent;
[0375] 3.5 parts of acid scavenger;
[0376] 0.2 parts of antioxidant;
[0377] Light stabilizer 0.15 parts;
[0378] Coupling agent KH171 0.4 parts.
[0379] Comparative Example 13
[0380] A method for preparing an acid scavenger is the same as that in specific embodiment 1.
[0381] An anti-PID EVA film for photovoltaic encapsulation material comprises the following raw materials in parts by weight:
[0382] EVA resin 100 parts;
[0383] 1.0 part of cross-linking agent;
[0384] 3.5 parts of acid scavenger;
[0385] 0.2 parts of antioxidant;
[0386] Light stabilizer 0.15 parts;
[0387] Coupling agent KH171 0.4 parts.
[0388] The physical properties of the EVA films prepared in Examples 1-17 of the present invention and Comparative Examples 1-13 were measured respectively, and the results are shown in Table 1.
[0389] Table 1 Physical test performance of each embodiment
[0390]
[0391]
[0392] First, it can be concluded from Examples 1-17 in Table 1 that the PID-resistant EVA film for photovoltaic encapsulation materials of the present invention has obvious advantages in adsorbing free acetic acid and resisting PID, and also has better optical properties.
[0393] Second, it can be observed from Example 1 and Comparative Examples 1-8 that the EVA film of the present invention has excellent free acetic acid adsorption and anti-PID performance using the homemade acid scavenger. Crown ethers, phosphates and hydroxyls (reaction products of epoxy groups and amino groups) have a positive effect on sodium ion adsorption; structures such as alkaline metal oxides, amino groups, and epoxy groups also play an important role in favoring the adsorption of acetic acid; at the same time, the structures work synergistically with each other to improve the adsorption effect of free acetic acid and the anti-PID effect.
[0394] Third, it can be observed from Example 1 and Comparative Examples 9-10 that the structure of the crown ether has a great influence on the adsorption effect; suitable crown ether pores have high adsorption capacity for sodium ions.
[0395] Fourth, it can be observed from Example 1 and Comparative Example 11 that the homemade acid scavenger of the present invention has a better effect than physical blending and chemical synthesis.
[0396] Fifth, it can be observed from Example 1 and Comparative Examples 12-13 that, through optimization of the formulation design, a reasonable cross-linking density has a positive effect on improving the performance of the product.
[0397] In summary, the acid-binding EVA encapsulation film of the present invention uses a homemade acid scavenger, has excellent acid removal effect, anti-PID performance, and also has excellent optical properties.
[0398] The test method is as follows:
[0399] (1) Free acid content: The ratio of the peak area of the carbonyl group to the carboxyl group is measured by ATR, P = A2 (1760 cm -1 :-C=O free acetic acid) / A1(1760cm -1 :-C=O free acetic acid); "A1" represents before aging test; "A2" represents after aging test. Aging conditions are: +85℃, relative humidity 85%, and test time is 720hr.
[0400] (2) Light transmittance: Tested according to the method described in GB / T 29848-2013 “Ethylene-vinyl acetate copolymer (EVA) adhesive film for photovoltaic module encapsulation”.
[0401] (3) Cross-linking degree: After the EVA film undergoes cross-linking reaction, the cross-linking degree is determined by xylene extraction. The EVA film is cut into 1 mm pieces, weighed as m0, and placed in a stainless steel mesh bag. It is immersed in boiling xylene and extracted for 4 hours. The uncross-linked EVA will be extracted into the xylene, and the remaining undissolved EVA is the cross-linked EVA film m1.
[0402] Crosslinking degree = crosslinked EVA film m1 / EVA total weight m0×100%
[0403] (4) PID power attenuation: The PID of the photovoltaic module is tested according to the industry standard IEC-62804. The test conditions are: 1500V voltage, 85°C, 85% relative humidity, and 192h.
[0404] (5) Resistance to humidity and heat aging: The EVA film was subjected to a humidity and heat aging test. Conditions: Test conditions: +85°C, relative humidity 85%, test time 1000 hours.
[0405] The visible light transmittance before and after the test was measured, and the visible light transmittance retention rate was calculated according to the following formula:
[0406] Retention rate of visible light transmittance=average light transmittance after the test / average light transmittance before the test×100%.
[0407] (6) UV aging resistance: The obtained EVA film was subjected to UV irradiation aging test according to the requirements of the International Electrotechnical Commission standard IEC61345. Test conditions: the surface temperature of the test piece is 60±5℃, the UV wavelength range is 280-400nm, and the irradiation intensity is 15kW·h / m 2 , the UV irradiation test time is 2000hr.
[0408] The visible light transmittance before and after the test was measured, and the visible light transmittance retention rate was calculated according to the following formula:
[0409] Retention rate of visible light transmittance=average light transmittance after the test / average light transmittance before the test×100%.
[0410] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A PID-resistant EVA film for photovoltaic encapsulation materials, characterized in that: The invention comprises the following raw materials in parts by weight: EVA resin 100 parts; Cross-linking agent 0.8-1.3 parts; 1.2-1.8 parts of auxiliary cross-linking agent; 2.5-4.5 parts of acid scavenger; Antioxidant 0.1-0.3 parts; Light stabilizer 0.1-0.2 parts; Coupling agent 0.3-0.5 parts; The preparation method of the acid scavenger comprises the following steps: Step S11, placing the nano-alkaline metal oxide and the silane coupling agent in an alcohol solvent to carry out a silanization coupling reaction to obtain a silane-modified metal oxide; Step S12, copolymerizing the olefin derivative and choline containing a carbon-carbon double bond under the action of a thermal initiator to obtain a polymer containing a choline structure; and Step S13, adding the polymer containing choline structure into acetone, stirring and fully dissolving; adding silane-modified metal oxide and crown ether into methanol solvent, ultrasonically dispersing for 0.5h, and standing; dropping the acetone solution of the polymer containing choline structure into the methanol system, ultrasonically dispersing evenly, and volatilizing naturally at room temperature to obtain the target product, i.e., the acid scavenger; The silane coupling agent is an aminosilane coupling agent; and The dosage ratio of the nano alkaline metal oxide, the silane coupling agent and the alcohol solvent is 1g: 3.5-5.5g: 80mL; The olefin derivative is an epoxide olefin or an amino olefin; and The choline containing a carbon-carbon double bond is a choline structure containing a carbon-carbon double bond and a phosphate; The usage ratio of the olefin derivative and the choline containing a carbon-carbon double bond is 3.0-5.0 mol: 5.0-7.0 mol; and The amount of the thermal initiator is 1.0-1.5% of the total mass of the reactants; The crown ether is 15-crown-5; The usage ratio of the silane-modified metal oxide, the polymer containing a choline structure and the crown ether is 4.5-6.5g: 5.0-5.5g: 4.0-5.0g.
2. The EVA film according to claim 1, characterized in that: The cross-linking agent is an organic peroxide cross-linking agent.
3. The EVA film according to claim 1, characterized in that: The auxiliary cross-linking agent is allyl and / or acryloxy.
4. The method for preparing the EVA film according to any one of claims 1 to 3, characterized in that: The steps include: S21, mixing, i.e. Adding raw materials into a mixer according to the formula ratio, mixing and stirring to obtain mixed raw materials; S22, extrusion, i.e. The mixed raw materials in S21 are placed in an extruder for melt blending, extrusion, casting, and cooling; as well as S23, film formation, i.e. After thickness measurement, edge pressing, shaping, edge trimming and rolling, the PID-resistant EVA film for photovoltaic encapsulation material is obtained.
Citation Information
Patent Citations
Anticorrosive photovoltaic packaging material EVA adhesive film and preparation method thereof
CN110093112A
Anti-PID functional additive, preparation method thereof and EVA adhesive film
CN117625082A