Heat-insulating glass containing functional coating and manufacturing method thereof
By using ATO/PU coatings made from modified polyurethane and modified ATO powder, the problems of insufficient dispersibility and UV resistance in heat-insulating glass were solved, achieving high-efficiency heat insulation and waterproof performance, and improving the stability and heat insulation effect of the glass.
Patent Information
- Application Number
- CN202410243527.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-03-04
AI Technical Summary
Existing heat-insulating glass has shortcomings in terms of dispersion and UV resistance, making it difficult to fully realize its heat insulation performance. In addition, water-based PU coatings have poor water resistance, which affects the stability and heat insulation effect of the glass.
ATO/PU coatings were prepared using modified polyurethane and modified ATO powder. The nano-ATO powder was uniformly dispersed by ball milling and then cross-linked and cured on the glass surface. Modified diols were used to improve the stability and UV resistance of the coatings.
It improves the light transmittance and heat insulation of the insulated glass, enhances the waterproof and UV-resistant properties of the coating, and ensures the stability and heat insulation effect of the glass.
Smart Images

Figure BDA0004725156160000031 
Figure BDA0004725156160000041 
Figure BDA0004725156160000042
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of heat-insulating glass, and in particular, relates to a heat-insulating glass containing a functional coating and a manufacturing method thereof. Background Art
[0002] In order to meet people's growing health needs, modern architectural designs mostly use full glass curtain walls, and some also open large skylights on the roof to enhance lighting and ventilation. With such a design, the lighting and ventilation of the building have indeed been greatly improved. However, this is accompanied by an increase in indoor radiation, an increase in indoor air conditioning load in summer, and an increase in building energy consumption. Therefore, improving the heat insulation of glass and ensuring light transmittance is an effective way to reduce building energy consumption.
[0003] The solar spectrum can be divided into three bands according to wavelength: ultraviolet, visible light, and infrared bands. Among them, infrared contains the largest radiation energy. Blocking infrared and ensuring the transmittance of visible light is the basic requirement of thermal insulation glass. At present, architectural thermal insulation glass mainly includes hollow glass, vacuum glass, Low-E glass, sunlight control glass, film glass, etc. These glasses are difficult to be used on a large scale due to the complex process of some and the high price of some. ATO (nano antimony tin oxide) is a common semiconductor material with good visible light transmittance and infrared blocking properties. Nano ATO can be added to water-based PU (polyurethane) as a functional powder to prepare a transparent thermal insulation coating. This coating has a wide range of applications in the fields of architectural glass and automotive glass. However, the dispersibility of nano ATO is poor, and the thermal insulation performance is difficult to fully exert; not only that, the water-based PU has poor waterproofness, and the coating will be damaged in humid and rainy days, resulting in performance degradation. In addition, there is currently little research on the anti-ultraviolet performance of thermal insulation glass, and its anti-ultraviolet performance needs to be improved to meet its higher demand in the field of thermal insulation glass. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a heat-insulating glass containing a functional coating and a manufacturing method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for manufacturing heat-insulating glass containing a functional coating comprises the following steps:
[0007] A1. Under nitrogen protection, add MDI (4,4'-diphenylmethane diisocyanate), dibutyltin dilaurate (catalyst), PPG (polypropylene glycol), modified diol, HO-PDMS (hydroxyl-terminated polydimethylsiloxane) and acetone to a three-necked flask equipped with a mechanical stirrer and reflux device, stir and mix evenly, and react at 45°C for 2h; then drop BDO (1,4-butanediol, chain extender) and react at 50°C for 2h; add azobisisobutyronitrile (initiator) and heat to 65°C, drop methacrylic acid and react for 4h; add HEA (hydroxyethyl acrylate, end-capping agent) and react at 45°C for 3h; add deionized water, emulsify at high speed shear for 75min, and remove acetone by vacuum rotary evaporation to obtain modified polyurethane;
[0008] A2, nano ATO powder was mixed with deionized water, KH570 (methacryloxypropyltrimethoxysilane) and agate beads (ball milling aid) were added, and the mixture was dispersed by ball milling at 480 r / min for 48 h in an agate tank to obtain modified ATO;
[0009] A3. Modified polyurethane, modified ATO and BPO (benzoyl peroxide, crosslinking agent) are mixed to obtain ATO / PU coating, which is evenly applied on the glass surface and placed in an oven at 85° C. for curing for 4 hours to obtain insulating glass containing a functional coating.
[0010] Furthermore, in step A1, the ratio of the amount of MDI, dibutyltin dilaurate, PPG, modified diol, HO-PDMS, acetone, BDO, azobisisobutyronitrile, methacrylic acid, HEA, and deionized water is 10-15 g: 0.05 g: 16 g: 2-4 g: 2 g: 100 mL: 1 g: 0.3 g: 2 g: 5 g: 100 mL.
[0011] Furthermore, in step A2, the ratio of the amount of nano-ATO powder, deionized water, KH570, and agate beads is 10-15 g:100 mL:3 g:4 g.
[0012] Furthermore, in step A3, the ratio of the amount of the modified polyurethane solution, the modified ATO solution, and the BPO is 10g:10g:0.05g.
[0013] ATO has good visible light transmittance and infrared blocking properties, giving the insulating glass good light transmittance and thermal insulation properties; the ball milling method is used to make the nano ATO powder dispersed more evenly; by surface vinyl modification of ATO, it will undergo a cross-linking reaction with modified polyurethane during curing, thereby improving the stability of the ATO / PU coating and making the performance of the resulting insulating glass more stable.
[0014] Further, the modified diol is prepared by the following steps:
[0015] S1. In a three-necked flask equipped with a stirring device, 2,2,6,6-tetramethylpiperidinol, n-octane and molybdenum trioxide were mixed and stirred uniformly, heated to 85°C, and tert-butyl hydroperoxide aqueous solution was added dropwise. After the addition was completed, the reaction was refluxed for 10 hours, filtered with suction, and the filtrate was added with activated carbon and stirred for 1 hour. The mixture was allowed to stand, filtered with suction, and the filtrate was taken. The n-octane was removed by distillation under reduced pressure to obtain intermediate 1; the ratio of the amount of 2,2,6,6-tetramethylpiperidinol, n-octane, molybdenum trioxide and tert-butyl hydroperoxide aqueous solution was 15.7g:15.8g:0.4g:10.3g;
[0016] Under the catalysis of molybdenum trioxide and the oxidation of tert-butyl hydroperoxide, 2,2,6,6-tetramethylpiperidinol and n-octane undergo a free radical coupling reaction; n-octane participates in the reaction process as a reactant and also acts as a reaction solvent, which can reduce the formation of by-products to obtain intermediate 1; the specific reaction process is as follows:
[0017]
[0018] S2. Add 1,3-acetone dicarboxylic acid, DAST (diethylaminosulfur trifluoride, fluorination reagent) and dichloromethane into a beaker, stir and mix evenly at room temperature, react for 40 minutes, filter, take the filter cake, wash it with anhydrous ethanol for 3 times, and dry it to obtain intermediate 2; the ratio of 1,3-acetone dicarboxylic acid, DAST and dichloromethane is 14.6 g:8.5 g:50 mL;
[0019] Under the action of the fluorination reagent, the carbonyl group on 1,3-acetone dicarboxylic acid is converted into a difluorinated compound. The fluorination reagent is selective and the carboxyl group is not affected, thereby obtaining intermediate 2. The specific reaction process is as follows:
[0020]
[0021] S3. In a three-necked flask equipped with a stirring device, the intermediate 1, the intermediate 2 and the pyridine were mixed and stirred uniformly, and dibutyltin oxide (catalyst) and DCC (dicyclohexylcarbodiimide, dehydrating agent) were added, and the reaction was carried out at 80° C. for 3 hours. After the reaction was completed, most of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 3; the ratio of the amount of intermediate 1, intermediate 2, pyridine, dibutyltin oxide and DCC was 18.7 g: 28.5 g: 100 mL: 0.5 g: 20.6 g;
[0022] Under the action of dibutyltin oxide and DCC, the carboxyl group on intermediate 2 and the hydroxyl group on intermediate 1 undergo esterification reaction. By controlling the molar ratio of the two to be close to 1:1 and the intermediate 1 to be slightly excessive, only one carboxyl group on intermediate 1 participates in the reaction to obtain intermediate 3. The specific reaction process is as follows:
[0023]
[0024] S4. In a three-necked flask equipped with a stirring device, the intermediate 3, serinol, DCC (dehydrating agent) and pyridine were mixed and stirred evenly, and the mixture was reacted for 75 min in a 60°C water bath. After the reaction, part of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol in a volume ratio of 3:7), and the eluent was removed by rotary evaporation to obtain a modified diol; the ratio of the amount of intermediate 3, serinol, DCC and pyridine was 43.5 g:9.1 g:20.6 g:200 mL;
[0025] The amino group of serinol and the carboxyl group of intermediate 3 undergo an amidation reaction, and under the action of a dehydrating agent, the reaction can be carried out under relatively mild conditions to obtain a modified diol. The specific reaction process is as follows:
[0026]
[0027] The prepared modified diol can directly participate in the polymerization reaction of polyurethane, so that ATO / PU coating has long-lasting performance; hindered amine plays the role of light stabilizer, decomposing hydrogen dioxide to produce stable nitroxide free radicals in light protection, this compound can very effectively capture the free radicals produced in photo-oxidative degradation, can effectively inhibit the photo-oxidative degradation of ATO / PU coating, and can be regenerated under stable conditions, giving ATO / PU coating stable and efficient anti-ultraviolet performance; CF bond has a very strong bond energy, the higher the chemical bond energy, the better the stability, further improving the ATO / PU coating The stability of ATO / PU coating can be improved, and at the same time, it can give ATO / PU coating excellent water resistance. Moreover, the CF bond will gradually migrate to the surface of ATO / PU coating, making ATO / PU coating have very low surface energy; in addition, the CF bond will well cover the CC main chain, shield it, and play a protective role, so that the stability of ATO / PU coating can be further improved; in addition, the ester group and amide group contained in the modified diol have certain hydrophobic properties; finally, the long carbon chain in the modified diol not only has certain hydrophobicity, but also can be inserted into the polyurethane molecule to improve stability.
[0028] It should be added that HO-PDMS and modified diols can play a joint modification role of fluorine and silicon, adjusting the surface wettability of polyurethane to superhydrophobicity, which can significantly enhance the hydrophobicity of polyurethane and thus improve the waterproof performance of ATO / PU coatings.
[0029] Beneficial effects of the present invention:
[0030] The heat-insulating glass of the present invention is made of modified polyurethane and modified ATO, and the ATO / PU coating is applied on the glass surface and cross-linked and cured under the action of a cross-linking agent. The modified polyurethane raw material contains modified diol, which can give the coating stable and efficient waterproof performance, UV resistance and a certain degree of impact resistance; the modified ATO is obtained by ball milling, so that the nano ATO powder is dispersed more evenly, so that the performance of ATO can be fully exerted, and the heat-insulating glass is given good light transmittance and heat insulation; finally, cross-linking and curing can further improve the stability of the heat-insulating glass. Therefore, the obtained heat-insulating glass has good light transmittance and strong heat insulation, and the coating also has stable and efficient waterproof performance and UV resistance, which has important application significance in the field of heat-insulating glass. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] Preparation of modified diols
[0034] S1. In a three-necked flask equipped with a stirring device, 15.7 g of 2,2,6,6-tetramethylpiperidinol, 15.8 g of n-octane and 0.4 g of molybdenum trioxide were mixed and stirred evenly, heated to 85°C, and 10.3 g of tert-butyl hydroperoxide aqueous solution (mass fraction 70%) was added dropwise. After the addition was completed, the reaction was refluxed for 10 h, filtered, activated carbon was added to the filtrate, stirred for 1 h, allowed to stand, filtered, the filtrate was taken, and n-octane was removed by vacuum distillation to obtain intermediate 1;
[0035] S2, add 14.6 g of 1,3-acetone dicarboxylic acid, 8.5 g of DAST and 50 mL of dichloromethane into a beaker, stir and mix evenly at room temperature, react for 40 min, filter, take the filter cake, wash it with anhydrous ethanol for 3 times, and dry it to obtain intermediate 2;
[0036] S3, in a three-necked flask equipped with a stirring device, 18.7 g of intermediate 1, 28.5 g of intermediate 2 and 100 mL of pyridine were mixed and stirred evenly, 0.5 g of dibutyltin oxide and 20.6 g of DCC were added, and the mixture was reacted at 80°C for 3 h. After the reaction was completed, most of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0037] S4. In a three-necked flask equipped with a stirring device, 43.5 g of intermediate 3, 9.1 g of serinol, 20.6 g of DCC and 200 mL of pyridine were mixed and stirred evenly, and reacted for 75 min in a 60°C water bath. After the reaction, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol in a volume ratio of 3:7), and the eluent was removed by rotary evaporation to obtain a modified diol.
[0038] Example 2
[0039] Preparation of modified diols
[0040] S1. In a three-necked flask equipped with a stirring device, 31.4 g of 2,2,6,6-tetramethylpiperidinol, 31.6 g of n-octane and 0.8 g of molybdenum trioxide were mixed and stirred evenly, heated to 85°C, and 20.6 g of tert-butyl hydroperoxide aqueous solution (mass fraction 70%) was added dropwise. After the addition was completed, the reaction was refluxed for 10 h, filtered, activated carbon was added to the filtrate, stirred for 1 h, allowed to stand, filtered, the filtrate was taken, and n-octane was removed by vacuum distillation to obtain intermediate 1;
[0041] S2. Add 29.2 g of 1,3-acetone dicarboxylic acid, 17 g of DAST and 100 mL of dichloromethane into a beaker, stir and mix evenly at room temperature, react for 40 min, filter, take the filter cake, wash it with anhydrous ethanol for 3 times, and dry it to obtain intermediate 2;
[0042] S3, in a three-necked flask equipped with a stirring device, 37.4 g of intermediate 1, 57 g of intermediate 2 and 200 mL of pyridine were mixed and stirred evenly, 1 g of dibutyltin oxide and 20.6 g of DCC were added, and the mixture was reacted at 80°C for 3 h. After the reaction was completed, most of the solvent was first removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0043] S4. In a three-necked flask equipped with a stirring device, 43.5 g of intermediate 3, 9.1 g of serinol, 20.6 g of DCC and 200 mL of pyridine were mixed and stirred evenly, and reacted for 75 min in a 60°C water bath. After the reaction, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of ethyl acetate / methanol in a volume ratio of 3:7), and the eluent was removed by rotary evaporation to obtain a modified diol.
[0044] Example 3
[0045] A1. Under nitrogen protection, 10 g of MDI, 0.05 g of dibutyltin dilaurate, 16 g of PPG (molecular weight 400), 2 g of the modified diol prepared in Example 1, 2 g of HO-PDMS and 100 mL of acetone were added to a three-necked flask equipped with a mechanical stirrer and a reflux device, and the mixture was stirred and mixed evenly. The mixture was reacted at 45° C. for 2 h. 1 g of BDO was added dropwise and the mixture was reacted at 50° C. for 2 h. 0.3 g of azobisisobutyronitrile was added and the temperature was raised to 65° C. 2 g of methacrylic acid was added dropwise and the mixture was reacted for 4 h. 5 g of HEA was added and the mixture was reacted at 45° C. for 3 h. 100 mL of deionized water was added and the mixture was emulsified at high speed for 75 min. The acetone was removed by vacuum rotary evaporation to obtain a modified polyurethane.
[0046] A2, 10g of nano ATO powder was mixed with 100mL of deionized water, 3g of KH570 and 4g of agate beads were added, and the mixture was dispersed by ball milling at 480r / min in an agate pot for 48h to obtain modified ATO;
[0047] A3. Mix 10 g of modified polyurethane, 10 g of modified ATO and 0.05 g of BPO to obtain ATO / PU coating, apply it evenly on the glass surface, place it in an oven at 85° C. for curing for 4 hours, and obtain insulating glass with functional coating.
[0048] Example 4
[0049] A1. Under nitrogen protection, 15 g of MDI, 0.05 g of dibutyltin dilaurate, 16 g of PPG (molecular weight 400), 3 g of the modified diol prepared in Example 2, 2 g of HO-PDMS and 100 mL of acetone were added to a three-necked flask equipped with a mechanical stirrer and a reflux device, and the mixture was stirred and mixed evenly. The mixture was reacted at 45° C. for 2 h. 1 g of BDO was added dropwise and the mixture was reacted at 50° C. for 2 h. 0.3 g of azobisisobutyronitrile was added and the temperature was raised to 65° C. 2 g of methacrylic acid was added dropwise and the mixture was reacted for 4 h. 5 g of HEA was added and the mixture was reacted at 45° C. for 3 h. 100 mL of deionized water was added and the mixture was emulsified at high speed for 75 min. The acetone was removed by vacuum rotary evaporation to obtain a modified polyurethane.
[0050] A2, 12g of nano ATO powder was mixed with 100mL of deionized water, 3g of KH570 and 4g of agate beads were added, and the mixture was dispersed by ball milling at 480r / min in an agate pot for 48h to obtain modified ATO;
[0051] A3. Mix 10 g of modified polyurethane, 10 g of modified ATO and 0.05 g of BPO to obtain ATO / PU coating, apply it evenly on the glass surface, place it in an oven at 85° C. for curing for 4 hours, and obtain insulating glass with functional coating.
[0052] Example 5
[0053] A1. Under nitrogen protection, 15 g of MDI, 0.05 g of dibutyltin dilaurate, 16 g of PPG (molecular weight 400), 4 g of the modified diol prepared in Example 2, 2 g of HO-PDMS and 100 mL of acetone were added to a three-necked flask equipped with a mechanical stirrer and a reflux device, and the mixture was stirred and mixed evenly. The mixture was reacted at 45° C. for 2 h; 1 g of BDO was added dropwise, and the mixture was reacted at 50° C. for 2 h; 0.3 g of azobisisobutyronitrile was added, the temperature was raised to 65° C., 2 g of methacrylic acid was added dropwise, and the mixture was reacted for 4 h; 5 g of HEA was added, and the mixture was reacted at 45° C. for 3 h; 100 mL of deionized water was added, and high-speed shear emulsification was performed for 75 min. The acetone was removed by vacuum rotary evaporation to obtain a modified polyurethane;
[0054] A2, 15g of nano-ATO powder was mixed with 100mL of deionized water, 3g of KH570 and 4g of agate beads were added, and the mixture was dispersed by ball milling at 480r / min in an agate pot for 48h to obtain modified ATO;
[0055] A3. Mix 10 g of modified polyurethane, 10 g of modified ATO and 0.05 g of BPO to obtain ATO / PU coating, apply it evenly on the glass surface, place it in an oven at 85° C. for curing for 4 hours, and obtain insulating glass with functional coating.
[0056] Comparative Example 1
[0057] No modified diol was added, and the remaining steps were the same as in Example 5.
[0058] Comparative Example 2
[0059] Use the building exterior wall thermal insulation paint produced by Guangzhou Bijiasuo Building Materials Co., Ltd. to apply the same glass as in Example 5.
[0060] The insulating glasses of Examples 3-5 and Comparative Examples 1-2 were made into corresponding shapes to be tested according to different test standards, and the following performance tests were performed:
[0061] The water resistance is measured using the national standard GB / T 1733-1993 "Determination of water resistance of paint films";
[0062] Adopt national standard GB / T 1720-1989 "Determination of paint film adhesion" to measure adhesion;
[0063] The national standard GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics" is used to measure the light transmittance;
[0064] The national standard GB / T 2680-2021 is used to measure the ultraviolet absorbance (wavelength 200-420);
[0065] A square foam insulation box with a side length of 20 cm and an opening at the top was used. The insulating glass of Examples 3-5 and Comparative Examples 1-2 was made into a shape slightly larger than the opening at the top and placed on the top. A 500W infrared lamp similar to the infrared spectrum of the sun was used as the light source. The sample was 30 cm away from the light source and irradiated for 2 hours. The temperature change in the box before and after irradiation was recorded, which was δT.
[0066] The measured results are shown in the following table:
[0067]
[0068] It can be seen from the above table that the prepared insulating glass has good light transmittance and strong heat insulation. The coating also has stable and efficient waterproof and UV resistance, and has important application significance in the field of insulating glass.
[0069] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0070] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for manufacturing heat-insulating glass containing a functional coating, characterized in that: The following steps are involved: A1. Under nitrogen protection, 4,4'-diphenylmethane diisocyanate, dibutyltin dilaurate, polypropylene glycol, modified diol, hydroxyl-terminated polydimethylsiloxane and acetone were stirred and mixed evenly, and reacted at 45°C for 2h; 1,4-butanediol was added dropwise, and reacted at 50°C for 2h; azobisisobutyronitrile was added, the temperature was raised to 65°C, methacrylic acid was added dropwise, and reacted for 4h; hydroxyethyl acrylate was added, and reacted at 45°C for 3h; deionized water was added, high-speed shear emulsification was performed for 75min, and vacuum rotary evaporation was performed to obtain modified polyurethane; A2, mixing nano ATO powder with deionized water, adding KH570 and agate beads, and dispersing them in an agate tank by ball milling at 480r / min for 48h to obtain modified ATO; A3, mixing modified polyurethane, modified ATO and BPO to obtain ATO / PU coating, applying it evenly on the glass surface, placing it in an oven at 85° C. for curing for 4 hours, and obtaining heat-insulating glass containing functional coating; Wherein, the modified diol described in step A1 is prepared by the following steps: S1. Mix 2,2,6,6-tetramethylpiperidinol, n-octane and molybdenum trioxide and stir evenly, heat to 85°C, add tert-butyl hydroperoxide aqueous solution dropwise, reflux for 10 hours, filter with suction, add activated carbon to the filtrate and stir for 1 hour, let stand, filter with suction, take the filtrate, and distill under reduced pressure to obtain intermediate 1; S2, 1,3-acetone dicarboxylic acid, diethylamino sulfur trifluoride and dichloromethane were stirred and mixed at room temperature, reacted for 40 minutes, filtered, the filter cake was taken, washed with anhydrous ethanol for 3 times, and dried to obtain intermediate 2; S3, mixing intermediate 1, intermediate 2 and pyridine, adding dibutyltin oxide and dicyclohexylcarbodiimide, reacting at 80°C for 3h, rotary evaporation, column chromatography purification, rotary evaporation to obtain intermediate 3; S4. The intermediate 3, serinol, DCC and pyridine were mixed and stirred evenly, placed in a 60° C. water bath, reacted for 75 min, and subjected to rotary evaporation. The mixture was purified by column chromatography and rotary evaporation to obtain a modified diol.
2. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step S1, the ratio of the amount of 2,2,6,6-tetramethylpiperidinol, n-octane, molybdenum trioxide, and tert-butyl hydroperoxide aqueous solution is 15.7 g: 15.8 g: 0.4 g: 10.3 g.
3. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step S2, the ratio of 1,3-acetonedicarboxylic acid, diethylaminosulfur trifluoride, and dichloromethane is 14.6 g:8.5 g:50 mL.
4. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step S3, the ratio of the amount of intermediate 1, intermediate 2, pyridine, dibutyltin oxide and dicyclohexylcarbodiimide is 18.7 g: 28.5 g: 100 mL: 0.5 g: 20.6 g.
5. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step S4, the ratio of the amount of intermediate 3, serinol, DCC, and pyridine is 43.5 g:9.1 g:20.6 g:200 mL.
6. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step A1, the ratio of 4,4'-diphenylmethane diisocyanate, dibutyltin dilaurate, polypropylene glycol, modified diol, hydroxyl-terminated polydimethylsiloxane, acetone, 1,4-butanediol, azobisisobutyronitrile, methacrylic acid, hydroxyethyl acrylate, and deionized water is 10-15g:0.05g:16g:2-4g:2g:100mL:1g:0.3g:2g:5g:100mL.
7. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step A2, the ratio of the amount of nano-ATO powder, deionized water, KH570, and agate beads is 10-15 g:100 mL:3 g:4 g.
8. The method for manufacturing a heat-insulating glass containing a functional coating according to claim 1, characterized in that: In step A3, the ratio of modified polyurethane, modified ATO and BPO used is 10g:10g:0.05g.
9. A heat-insulating glass with a functional coating, characterized in that: Made according to the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Water-based nano heat insulating coating used for glass and preparation method thereof
CN101538444A
Method for preparing nanometer ATO dispersing slurry fast, efficiently and cheaply
CN101948635A
Waterborne fluorine-containing polyurethane resin capable of being cured by UV (Ultraviolet) and preparation method of waterborne fluorine-containing polyurethane resin
CN104231228A
Preparation method for UV (Ultraviolet)-curable WPU (Waterborne Polyurethane) high heat-insulating coating
CN109666105A
Preparation method of light-cured waterborne polyurethane acrylate adhesive
CN116376506A