A fabric stiffening agent and preparation method thereof

By copolymerizing acrylate prepolymer with styrene monomer and adding thiol cross-linking agent, a dense network structure is formed, which solves the problems of slow curing speed of existing fabric stiffeners and difficulty in improving water resistance and gloss, and realizes fabric Rapid curing and overall performance improvement of stiffeners.

CN118165196BActive Publication Date: 2024-10-11GUANGDONG RUNXIANG FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410373136.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-11
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

When existing fabric stiffeners are used to improve water resistance and gloss, the curing speed is slow, and it is difficult to improve water resistance and gloss at the same time.

Method used

Acrylate prepolymer is copolymerized with styrene monomer, and a thiol cross-linking agent is added during the prepolymerization process to adjust the viscosity and stability of the emulsion, reduce the tendency of monomer self-polymerization, form a dense network structure, and improve water resistance and Cure speed.

Benefits of technology

It achieves the comprehensive properties of fast curing, excellent gloss and water resistance of fabric stiffening agent, and the stiffening performance is improved with the addition of a smaller amount of styrene monomer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004766201690000041
    Figure BDA0004766201690000041
  • Figure BDA0004766201690000051
    Figure BDA0004766201690000051
Patent Text Reader

Abstract

The present invention provides a fabric stiffener and a preparation method thereof. The fabric stiffener of the present invention comprises the following components in parts by weight: 322-525 parts of acrylate prepolymer, 15-75 parts of styrene, 1-6 parts of acrylic acid, 3-8 parts of emulsifier, 15-30 parts of polyvinyl alcohol, 0.2-0.5 parts of initiator, and 360-600 parts of water; wherein the acrylate prepolymer comprises the following reaction raw materials in parts by weight: 300-450 parts of vinyl acetate, 15-45 parts of methyl methacrylate, 3-10 parts of versatate vinyl carbonate, 3-10 parts of acrylic acid, 1-3 parts of initiator, and 1-10 parts of thiol crosslinking agent. The present invention first prepares the acrylate monomer into a prepolymer, and then copolymerizes it with a styrene monomer, and at a relatively small amount of polyvinyl alcohol and styrene monomer added, the gloss and water resistance of the prepared fabric stiffener are improved, and the curing speed is relatively fast.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printing and dyeing auxiliaries, in particular to a fabric stiffening agent and a preparation method thereof. Background Art

[0002] Fabric stiffening is an important style finishing. After stiffening, the textiles can obtain a rigid, crisp, elastic and thick hand feeling style. It is mainly used in the finishing process of curtains, bags, workwear, knitted fabrics and other fabrics. The commonly used stiffening agents on the market are: melamine resin, urea-formaldehyde resin, polyacrylate emulsion, polystyrene-acrylic emulsion, polyvinyl acetate-acrylic emulsion, white latex (polyvinyl acetate emulsion), etc.

[0003] White latex stiffener is a kind of milky white viscous emulsion obtained by graft polymerization of vinyl acetate monomer and polyvinyl alcohol under the conditions of emulsifier, initiator and heating. A small amount of it can achieve excellent stiffening effect, so it is widely used. As an important raw material in the stiffener, polyvinyl alcohol needs to be added in a certain amount to prevent sagging and improve the appearance performance (such as gloss) after the stiffener is applied; however, if the amount of polyvinyl alcohol added is too large, the molecular weight of the matrix obtained after the monomer polymerization will be large, the viscosity will increase, the coating performance will deteriorate, the coating will be uneven, and the water resistance will be reduced. Therefore, it is difficult to improve the water resistance and gloss of the current white latex stiffener at the same time. At present, in order to improve the water resistance and weather resistance of the stiffener, styrene monomers are introduced into the stiffener, but the introduction of styrene monomers will reduce the curing speed of the stiffener resin matrix to a certain extent.

[0004] Therefore, it is necessary to develop a fabric stiffening agent with fast curing speed and excellent comprehensive performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a fabric stiffening agent which can be quickly cured and has excellent gloss, water resistance and stiffening properties.

[0006] Another object of the present invention is to provide a method for preparing the fabric stiffening agent.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] A fabric stiffening agent, comprising the following components in parts by weight:

[0009] 322-525 parts of acrylate prepolymer, 15-75 parts of styrene, 1-6 parts of acrylic acid, 3-8 parts of emulsifier, 15-30 parts of polyvinyl alcohol, 0.2-0.5 parts of initiator, 360-600 parts of water;

[0010] The acrylic ester prepolymer comprises the following reactive monomers in parts by weight: 300-450 parts of vinyl acetate, 15-45 parts of methyl methacrylate, 3-10 parts of vinyl versatate, 3-10 parts of acrylic acid, and 1-10 parts of a thiol crosslinking agent.

[0011] The present invention first prepares an acrylate monomer into a prepolymer, and then copolymerizes the prepolymer with a styrene monomer. The acrylate prepolymer can act together with polyvinyl alcohol to adjust the viscosity and stability of the stiffener emulsion. When a relatively small amount of polyvinyl alcohol is added, the stiffener can have good coating performance, and no phenomenon such as sagging will occur to affect the appearance of the fabric. At the same time, the present invention also adds a thiol cross-linking agent during the prepolymer prepolymerization process to reduce the self-polymerization tendency of vinyl acetate and methyl methacrylate in the acrylate monomer, which is conducive to obtaining a copolymer prepolymer. The hard monomer and the soft monomer chain segments are combined with each other to form a dense network structure with a certain strength, which can block the erosion of the stiffener by moisture to a certain extent, and can achieve higher water resistance when a relatively small amount of styrene monomer is added. The addition of a relatively small amount of styrene monomer can also increase the curing speed of the stiffener on the fabric surface.

[0012] Preferably, the method for preparing the acrylic ester prepolymer comprises the following steps: vinyl acetate, methyl methacrylate, vinyl versatate, acrylic acid, and a thiol crosslinking agent are reacted in the presence of an initiator at 80-90° C. for 0.5-1 h.

[0013] Preferably, the thiol crosslinking agent includes at least one of trimethylolpropane tris(3-mercaptopropionate), dithiodiphenyl ether, and dithiodiphenyl disulfide; more preferably, trimethylolpropane tris(3-mercaptopropionate).

[0014] The initiators used to prepare the fabric stiffener and the acrylic prepolymer can be the same or different, and the initiators are independently selected from peroxide initiators, including but not limited to at least one of ammonium persulfate, potassium persulfate, tert-butyl hydroperoxide, and hydrogen peroxide.

[0015] Preferably, the emulsifier includes but is not limited to at least one of disodium sulfosuccinate ethoxylate lauryl monoester, sodium allyloxyhydroxypropyl sulfonate, and vinyl sulfonic acid. The addition of the emulsifier can make the polyvinyl alcohol particles more uniform and have very good mechanical stability.

[0016] Preferably, the molecular weight of the polyvinyl alcohol is 500-3000. When the molecular weight of the polyvinyl alcohol is within this range, the size of the polymer particles can be kept within a suitable range, which is convenient for subsequent processing.

[0017] Corresponding functional additives may be added to the fabric stiffener as required. For example, the functional additive may be a reducing agent, which is used to adjust the pH in the fabric stiffener, especially when the pH is in the range of 5-6, the adhesion between the stiffener and the fabric is better. The reducing agent includes but is not limited to at least one of sodium bisulfite and sodium 2-methyl-4-nitrobenzene sulfinate.

[0018] The amount of the functional additive is controlled within the range of 0.1-0.3 parts by weight.

[0019] The present invention also provides a method for preparing the fabric stiffening agent, which specifically comprises the following steps:

[0020] S1. According to the parts by weight, polyvinyl alcohol and an emulsifier are dissolved in water to obtain a polyvinyl alcohol colloidal solution;

[0021] S2. Add the reaction raw material of the acrylic ester prepolymer to the polyvinyl alcohol colloidal solution obtained in step S1 at 75-85°C, and react at 80-90°C for 0.5-1h to obtain a colloidal solution containing an acrylic ester prepolymer;

[0022] S3. Add styrene, acrylic acid and initiator into water to obtain a second monomer reaction liquid, add the second monomer reaction liquid dropwise into the colloidal solution obtained in step S2 at 80-90° C., keep warm for 1-1.5 hours, and cool to room temperature to obtain the fabric stiffening agent.

[0023] Preferably, the dropping time in step S2 is 4-6 hours.

[0024] Preferably, the dropping time in step S3 is 0.5-1 h.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention first prepares acrylate monomers into prepolymers, and then copolymerizes the prepolymers with styrene monomers. The gloss, water resistance and stiffening performance of the prepared fabric stiffener can be improved while adding relatively small amounts of polyvinyl alcohol and styrene monomers, and the curing speed is relatively fast. DETAILED DESCRIPTION

[0027] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.

[0028] Examples 1-9

[0029] A series of fabric stiffening agents are provided, which are prepared according to the formula (parts by weight) shown in Table 1 and a method comprising the following steps:

[0030] S1. dissolving polyvinyl alcohol and an emulsifier in water to obtain a polyvinyl alcohol colloidal solution;

[0031] S2. At 85° C., adding the reaction raw material of the acrylic ester prepolymer to the polyvinyl alcohol colloidal solution obtained in step S1, and reacting at 90° C. for 0.5 h to obtain a colloidal solution containing an acrylic ester prepolymer;

[0032] S3. Add styrene, acrylic acid and initiator into water to obtain a second monomer reaction liquid. Add the second monomer reaction liquid dropwise into the colloidal solution obtained in step S2 at 80° C., keep warm for 1.5 hours, and cool to room temperature to obtain the fabric stiffening agent.

[0033] Table 1

[0034]

[0035] Comparative Example 1

[0036] This comparative example provides a fabric stiffening agent, which is prepared by referring to the method of Example 1, and is different from Example 1 in that no thiol cross-linking agent is added.

[0037] Comparative Example 2

[0038] This comparative example provides a fabric stiffening agent, which is prepared by referring to the method of Example 1, and differs from Example 1 in that methyl methacrylate is replaced by an equal mass of vinyl acetate.

[0039] Comparative Example 3

[0040] This comparative example provides a fabric stiffening agent, which has the same formulation as that in Example 1, except that the preparation method comprises the following steps:

[0041] S1. dissolving polyvinyl alcohol and an emulsifier in water to obtain a polyvinyl alcohol colloidal solution;

[0042] S2. Add the raw materials described in Table 1 into water to obtain a reaction solution, heat it to 90° C., react for 0.5 h, and cool it to room temperature to obtain the fabric stiffening agent.

[0043] Comparative Example 4

[0044] This comparative example provides a fabric stiffening agent, which is different from comparative example 3 in that the added amount of polyvinyl alcohol is increased to 35 parts by weight.

[0045] Comparative Example 5

[0046] This comparative example provides a fabric stiffening agent, which is different from comparative example 3 in that the added amount of polyvinyl alcohol is increased to 35 parts by weight, and the added amount of styrene is increased to 100 parts by weight.

[0047] Performance Testing

[0048] The fabric stiffening agent obtained in the above examples and comparative examples was dissolved in water and diluted to a concentration of 200 g / L. Then the polyester cloth was immersed in the stiffening agent solution and then fixed at 180° C. (and the fixing time was recorded in Table 2). After fixing, the following tests were performed:

[0049] 1. Stiffness (mm): Tested in accordance with GB / T 18318-2001 "Determination of bending length of textile fabrics". The test results (recorded as h1, mm) are shown in Table 2.

[0050] 2. Water resistance (%): The polyester treated with stiffener was placed in neutral water at 80°C for 10 minutes, and the stiffness of the washed fabric (polyester cloth treated with stiffener) was tested (recorded as h2, mm), and the stiffness change rate was calculated, stiffness change rate (%) = (h2-h1) / h1*100%, and the test results are shown in Table 2;

[0051] 3. Glossiness (%): tested using a glossiness tester, unit: %. Test results are shown in Table 2.

[0052] Table 2 Performance test results

[0053]

[0054] From the above results we can see that:

[0055] The fabric stiffener prepared by the invention has excellent comprehensive performance, can be quickly cured, and has excellent glossiness, water resistance and stiffness performance: wherein, the curing and setting time is within 92 seconds, and can be as low as 86 seconds; after being washed with water at 80°C, the stiffness change rate of the fabric is below 10%, and can be as low as 6%; the glossiness is above 68%, and can be as high as 73%.

[0056] In Comparative Example 1, no thiol crosslinking agent was added, and the monomer copolymerization stability of the acrylate prepolymer was poor, resulting in changes in the chain segments and crosslinking structure of the stiffening agent, which in turn resulted in poor water resistance of the fabric.

[0057] In Comparative Example 2, the monomers in the acrylic ester prepolymer were changed, resulting in a decrease in the density and strength of the cross-linked network of the stiffening agent, and the stiffness and water resistance of the fabric were deteriorated.

[0058] In Comparative Example 3, the acrylic ester monomers were not prepolymerized first, but all the reactive monomer raw materials were mixed and copolymerized together. The polymer cross-linked network structure of the obtained stiffening agent was different, and the performance of the obtained fabric was significantly deteriorated.

[0059] In Comparative Example 4, the acrylic ester monomer was not prepolymerized, but in order to improve the appearance performance of the fabric, the amount of polyvinyl alcohol added was increased. As can be seen from Table 2, the water resistance of the fabric was significantly deteriorated; and in order to further improve the water resistance of the fabric, the amount of styrene monomer added was further increased in Comparative Example 5. Although the water resistance and gloss of the fabric were improved, the setting time of the fabric after being treated with a stiffening agent was significantly increased.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A fabric stiffening agent, characterized in that: The composition comprises the following components in parts by weight: 322-525 parts of acrylate prepolymer, 15-75 parts of styrene, 1-6 parts of acrylic acid, 3-8 parts of emulsifier, 15-30 parts of polyvinyl alcohol, 0.2-0.5 parts of initiator, 360-600 parts of water; The acrylic ester prepolymer comprises the following reactive monomers in parts by weight: 300-450 parts of vinyl acetate, 15-45 parts of methyl methacrylate, 3-10 parts of vinyl versatate, 3-10 parts of acrylic acid, and 1-10 parts of a thiol crosslinking agent.

2. The fabric stiffening agent according to claim 1, characterized in that The preparation method of the acrylic ester prepolymer comprises the following steps: Vinyl acetate, methyl methacrylate, vinyl versatate, acrylic acid, and a thiol crosslinking agent are reacted in the presence of an initiator at 80-90° C. for 0.5-1 h.

3. The fabric stiffening agent according to claim 1, characterized in that The thiol crosslinking agent includes at least one of trimethylolpropane tris(3-mercaptopropionate), dithiodiphenyl ether, and dithiodiphenyl disulfide.

4. The fabric stiffening agent according to claim 1, characterized in that The initiator includes at least one of ammonium persulfate, potassium persulfate, tert-butyl hydroperoxide and hydrogen peroxide.

5. The fabric stiffening agent according to claim 1, characterized in that: The emulsifier includes at least one of disodium sulfosuccinate ethoxy ether lauryl monoester, sodium allyloxy hydroxypropyl sulfonate, and vinyl sulfonic acid.

6. The fabric stiffening agent according to claim 1, characterized in that: The molecular weight of the polyvinyl alcohol is 500-3000.

7. The fabric stiffening agent according to claim 1, characterized in that The fabric stiffening agent also includes 0.1-0.3 parts of functional additives, and the functional additives include reducing agents.

8. The fabric stiffening agent according to claim 7, characterized in that The reducing agent includes at least one of sodium bisulfite and sodium 2-methyl-4-nitrobenzene sulfinate.

9. The method for preparing the fabric stiffening agent according to any one of claims 1 to 8, characterized in that: The steps include: S1. According to the parts by weight, polyvinyl alcohol and an emulsifier are dissolved in water to obtain a polyvinyl alcohol colloidal solution; S2. Add the reaction raw material of the acrylic ester prepolymer to the polyvinyl alcohol colloidal solution obtained in step S1 at 75-85°C, and react at 80-90°C for 0.5-1h to obtain a colloidal solution containing an acrylic ester prepolymer; S3. Add styrene, acrylic acid and initiator into water to obtain a second monomer reaction liquid, add the second monomer reaction liquid dropwise into the colloidal solution obtained in step S2 at 80-90° C., keep warm for 1-1.5 hours, and cool to room temperature to obtain the fabric stiffening agent.

10. The preparation method according to claim 9, characterized in that: The time of dropping in step S2 is 4-6 hours; and / or the time of dropping in step S3 is 0.5-1 hour.