A PCR HIPS material for POSS machine and preparation method thereof

By adding K resin and optimized filler to the PCR HIPS material, the problem of insufficient anti-fall performance of recycling PCR HIPS on the POSS machine shell is solved, and materials with high impact resistance and aging resistance are prepared, realizing the Significant improvement in material performance.

CN118165455BActive Publication Date: 2024-11-08JIAN GUOHENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410285841.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-11-08
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

When used in POSS shells, the recycled PCR HIPS materials have low drop resistance and are prone to damage after long-term use. Due to the complex impurity components, they are insufficient scratch resistance and aging resistance.

Method used

Using PCR HIPS as the main resin material, K resin, filler, toughener, compatibilizer, stabilizer and antioxidant were added, and through uniform mixing and melt extrusion processes, high impact resistance, flexibility and Hardness material, optimize the compatibility of filler to improve material performance.

Benefits of technology

The PCR HIPS material produced has good drop resistance, scratch resistance and aging resistance. It is not easy to wear and discolor after long-term use, and has a long service life. It also improves the resistance through the synergy of modified filler and toughener. Impact strength and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004739109730000061
    Figure BDA0004739109730000061
  • Figure BDA0004739109730000071
    Figure BDA0004739109730000071
  • Figure BDA0004739109730000081
    Figure BDA0004739109730000081
Patent Text Reader

Abstract

The present application relates to the field of recycled HIPS materials, and specifically discloses a PCR HIPS material for a POSS machine and a preparation method thereof. A PCR HIPS material for a POSS machine is prepared from the following raw materials in parts by weight: 50-80 parts of PCR HIPS, 15-25 parts of K resin, 12-22 parts of filler, 4-8 parts of toughening agent, 3-8 parts of compatibilizer, 1-3 parts of lubricant, 2.5-4.5 parts of stabilizer, and 0.5-2 parts of antioxidant; preparation method: raw material mixing, melt extrusion, cooling, drying, and pelletizing. The PCR HIPS prepared in the present application has good impact resistance, flexibility, hardness, and aging resistance, and is applied to the POSS machine housing, and has good anti-fall performance, scratch resistance, and aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of recycled HIPS materials, and more specifically, to a PCRHIPS material for a POSS machine and a preparation method thereof. Background Art

[0002] High impact polystyrene, referred to as HIPS, is a polystyrene-modified non-crystalline material with high impact strength modified by synthetic rubber. It has good impact strength, toughness, material rigidity and processing performance. It is widely used in electronic appliances, optical lighting, mechanical equipment, building materials industry and other fields.

[0003] With the continuous development of the national economy and the continuous tightening of low-carbon emission policies, the requirements for low-carbon emission indicators for chemical materials are becoming higher and higher. In order to improve the utilization efficiency of high HIPS, HIPS has gradually begun to be recycled and reused as recycled HIPS material, referred to as PCR HIPS, to reduce carbon emissions.

[0004] When the recycled PCR HIPS is used in the POSS machine casing, it needs to have good scratch resistance, aging resistance and drop resistance. However, since HIPS products will age during use, and auxiliary materials such as ABS material, PP material or PE material are added during the production process of HIPS products, the impurity composition in the recycled PCR HIPS is more complex, resulting in low scratch resistance, aging resistance and drop resistance of the recycled PCR HIPS.

[0005] In order to improve the scratch resistance, aging resistance and drop resistance of the recycled PCR HIPS, reinforcing fillers are usually added. Although the addition of reinforcing fillers can greatly improve the scratch resistance of the recycled PCR HIPS, it will also increase the hardness of the recycled PCR HIPS, thereby reducing the drop resistance of the prepared POSS machine casing. It is still prone to damage after long-term use. Therefore, further improvements are needed. Summary of the invention

[0006] In order to solve the problem that the recycled PCR HIPS is used in the POSS machine housing, the prepared POSS machine housing has low anti-fall performance and is easily damaged after long-term use, the present application provides a PCR HIPS material for a POSS machine and a preparation method thereof.

[0007] In the first aspect, the present application provides a PCR HIPS material for a POSS machine, using the following technical solution:

[0008] A PCR HIPS material for a POSS machine is prepared from the following raw materials in parts by weight:

[0009] PCR HIPS 50-80 copies

[0010] K resin 15-25 parts

[0011] Filling 12-22 parts

[0012] Toughener 4-8 parts

[0013] 3-8 parts of compatibilizer

[0014] 1-3 parts lubricant

[0015] Stabilizer 2.5-4.5 parts

[0016] Antioxidant 0.5-2 parts.

[0017] By adopting the above technical scheme, the PCR HIPS material prepared in the present application has good impact resistance, flexibility, hardness and aging resistance. When used in POSS machines, it has good drop resistance, scratch resistance and aging resistance, and is not easy to wear and discolor after long-term use.

[0018] In the present application, the recycled PCR HIPS is used as the main resin material, and K resin is added to the PCR HIPS as a reinforcing resin material. The K resin is a styrene-butadiene modified resin, has good impact strength and flexibility, has good compounding stability with PCR HIPS, and can improve the impact resistance and flexibility of the prepared PCR HIPS material. The toughening agent plays a role in further reinforcing the main resin material. Under the action of the compatibilizer, the PCR HIPS, the K resin and the toughening agent are uniformly mixed, and the impact resistance and flexibility of the prepared PCR HIPS material are improved. The filler plays a role in reinforcing the mechanical properties of the PCR HIPS, and can further improve the rigidity and hardness of the PCR HIPS material, so that the prepared PCR HIPS material has good impact strength and flexibility, and also has good hardness, thereby improving the scratch resistance of the prepared PCR HIPS. The stabilizer has good stability, and can further mix and melt the various components, so that the filler and the PCR The compatibility between HIPS, K resin and toughening agent is better, the raw materials are more tightly combined, the lubricant reduces the friction between the components, so that the components can be evenly mixed and melted, further improving the material properties of the prepared PCR HIPS modified material, and the antioxidant improves the anti-aging performance of the prepared PCR HIPS modified material.

[0019] Preferably, the toughening agent is composed of SEBS, vinyl-terminated polydimethylsiloxane and polyoxypropylene triol in a weight ratio of (1-1.5):(0.4-0.8):(0.1-0.3).

[0020] By adopting the above technical scheme, SEBS is a linear triblock copolymer with polystyrene as the terminal segment and ethylene-butylene copolymer obtained by hydrogenating polybutadiene as the middle elastic block. It has good strength as well as good elasticity and wear resistance. Terminal vinyl polydimethylsiloxane is a vinyl-terminated silicone macromolecular structure with good flexibility and dispersibility, which can improve the molecular stretchability of SEBS in the resin system. At the same time, the silicone chain segment can improve the impact strength of the prepared PCR HIPS material. Polyoxypropylene triol is a plasticizer with good performance, which can cooperate with terminal vinyl polydimethylsiloxane and SEBS to further improve the impact strength and toughness of the prepared PCR HIPS material, while improving aging resistance and wear resistance.

[0021] Preferably, the filler is a modified filler, and the modified filler is made from the following raw materials in parts by weight:

[0022] Powder filler 40-60 parts

[0023] Silane coupling agent 0.5-2 parts Vinyl ester resin 0.5-2 parts

[0024] Allyl alcohol glycidyl ether 1-3 parts;

[0025] The powder filler is any one or a combination of white carbon black, kaolin, and talc, and the silane coupling agent is one or a combination of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, vinyltrimethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and γ-aminopropyltriethoxysilane.

[0026] Preferably, the modified filler is prepared by the following steps:

[0027] A1. Add 40-60 parts of powder filler to 80-120 parts of 50-85wt% ethanol aqueous solution, then add 0.5-2 parts of silane coupling agent, heat to 50-65°C for reaction, react for 1-2h, filter, and dry to obtain pretreated powder filler;

[0028] A2. Add 1-3 parts of allyl glycidyl ether to the pretreated powder filler, mix well, then add 0.5-2 parts of vinyl ester resin, heat to 60-80°C, knead and stir, stir for 30-60 minutes, and obtain a modified filler.

[0029] By adopting the above technical solution, in order to further improve the compatibility of the filler and reduce the reduction in impact strength and flexibility of the prepared PCR HIPS material due to increased hardness, the filler is optimized. In the present application, a silane coupling agent, allyl glycidyl ether and vinyl ester resin are used to modify the powder filler, wherein allyl glycidyl ether has a soft long-chain ether group segment, which can fully infiltrate the powder filler. Under the action of the silane coupling agent, the powder filler is uniformly dispersed, and then the vinyl ester resin is added to coat the powder filler. The vinyl ester resin is a flexible resin with a good cross-linking density, which can improve the flexibility, aging resistance and impact resistance of the prepared PCR HIPS material, and at the same time has a good synergistic effect with the toughening agent, which can further improve the compatibility between the components, thereby improving the performance of the prepared PCR HIPS material.

[0030] Preferably, the compatibilizer is any one of styrene-octene-glycidyl methacrylate copolymer and styrene-acrylonitrile-glycidyl methacrylate copolymer.

[0031] By adopting the above technical scheme, styrene-octene-glycidyl methacrylate copolymer can better improve the compatibility of impurity components in PCR HIPS with HIPS, toughening agent, compatibilizer, stabilizer and filler. Styrene-acrylonitrile-glycidyl methacrylate copolymer has better impact strength and heat resistance than polystyrene. It also contains glycidyl methacrylate group. Therefore, it can improve the mechanical properties of the prepared PCR HIPS while improving the compatibility of impurity components in PCR HIPS with K resin, toughening agent, stabilizer and filler.

[0032] Preferably, the stabilizer is composed of POE and a long-chain alkyl silane coupling agent in a weight ratio of 1:(0.2-0.6).

[0033] By adopting the above technical scheme and using a better ratio of POE and long-chain alkyl silane coupling agent as stabilizers, it can play a better compounding effect with toughening agents, fillers, K resins and PCR resins, further improving the bonding density of each component, thereby improving the impact strength, flexibility, wear resistance and aging resistance of the prepared PCR HIPS material.

[0034] Preferably, the lubricant is one or more combinations of pentaerythritol stearate, ethylene bisstearamide, zinc stearate, and triphenyl phosphate.

[0035] By adopting the above technical solution, the lubricant has good lubricity, can reduce the friction between the raw materials of PCR HIPS, K resin, toughening agent, stabilizer and filler, so that each raw material is fully dispersed and evenly melted, improves the processing performance, and enhances the comprehensive performance of the prepared PCR HIPS material.

[0036] Preferably, the antioxidant consists of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:(1.5-2.5).

[0037] By adopting the above technical scheme, the compound use of the above antioxidants has a good synergistic effect, which can better improve the antioxidant properties of the prepared PCR HIPS material, so that the PCR HIPS material has better anti-aging performance when used in the POSS machine, thereby improving the service life of the POSS machine.

[0038] In a second aspect, the present application provides a method for preparing a PCR HIPS material for a POSS machine, using the following technical solution:

[0039] A preparation method for a PCR HIPS material for a POSS machine comprises the following preparation steps:

[0040] S1, baking the PCR HIPS raw material to obtain the PCR HIPS processed material;

[0041] S2, adding PCR HIPS processing material, K resin, toughening agent, compatibilizer and stabilizer into the reaction equipment, stirring evenly, to obtain mixture A;

[0042] S3, adding filler, lubricant and antioxidant to mixture A, stirring evenly to prepare PCR HIPS mixture;

[0043] S4, melt-extrude the PCR HIPS mixture, cool, dry and pelletize to obtain the PCR HIPS material.

[0044] By adopting the above technical scheme, PCR HIPS is first baked to remove water molecules and low-boiling impurities in PCR HIPS, and the PCR HIPS processed material is formed after baking. Then, K resin, toughening agent, compatibilizer and stabilizer are added to the PCR HIPS processed material, mixed and stirred to make the components evenly dispersed and mixed, and then filler, lubricant and antioxidant are added. Under the further action of lubricant, compatibilizer and stabilizer, the raw materials are further compatible to form a PCR HIPS mixture with uniform dispersion and dense structure. Then, the PCR HIPS mixture is melt-extruded, cooled, dried and pelletized to obtain a PCR HIPS material with good mechanical properties.

[0045] Preferably, the baking temperature in step S1 is 70-80°C, and the baking time is 45-120 min; and the melting temperature in step S4 is 190-230°C.

[0046] By adopting the above technical scheme, the optimal baking temperature and time can volatilize the water molecules and low-boiling impurities in PCR HIPS to a large extent, thereby improving the mechanical properties of the prepared PCR HIPS material. The optimal melting temperature enables the PCR HIPS mixture to be evenly melted and extruded, thereby improving the processing stability of the PCR HIPS material.

[0047] In summary, this application has the following beneficial effects:

[0048] 1. The PCR HIPS material for POSS machine of the present application uses PCR HIPS as the main resin material, and compounded K resin, filler, toughening agent, compatibilizer and stabilizer as auxiliary materials. The prepared PCR HIPS material has good impact strength, flexibility, hardness and aging resistance. When applied to POSS machine, the prepared POSS machine shell has good drop resistance, scratch resistance and aging resistance, is not easy to change color and scratch after long-term use, and has a long service life.

[0049] 2. By modifying the powder filler with silane coupling agent, allyl glycidyl ether and vinyl ester resin, the scratch resistance of the PCR HIPS material can be improved while having good impact resistance and aging resistance.

[0050] 3. By using a better proportion of SEBS, terminal vinyl polydimethylsiloxane and polyoxypropylene triol as toughening agents, and a better proportion of POE and long-chain alkyl silane coupling agent as stabilizers, it can produce a better synergistic effect with K resin and filler, improve the compatibility of each component with PCR HIPS, and improve the impact strength, flexibility, hardness and aging resistance of the prepared PCR HIPS material. DETAILED DESCRIPTION

[0051] The present application is further described in detail below with reference to the embodiments.

[0052] The following are the sources and specifications of some raw materials of this application. The raw materials in the preparation examples and embodiments of this application can be obtained from the market. The raw materials used in this application include but are not limited to the specific models and manufacturers disclosed below. Raw materials with the same specifications and performance can be used:

[0053] 1. PCR HIPS: commercially available, cantilever beam notched impact strength: 60 J / m, heat deformation temperature 75 ° C, tensile strength 19.2 MPa, plastic waste recycling by Heilongjiang Zhongzai Waste Appliance Dismantling Co., Ltd.;

[0054] 2. K resin: Korea Dalin, model: KR03, injection molding grade;

[0055] 3. Styrene-octene-glycidyl methacrylate copolymer: Jiayirong brand, SOG-02;

[0056] 4. Styrene-acrylonitrile-glycidyl methacrylate copolymer: Jiayirong brand, SAG-005;

[0057] 5. SEBS: Brand: Kraton, styrene content 29-32%, model G1654;

[0058] 6. Vinyl-terminated polydimethylsiloxane: molecular weight 10000-20000, vinyl content 0.2-0.6%, viscosity 500-1000 (25°C, mpa·s);

[0059] 7. Polyoxypropylene triol: Model 330N, hydroxyl value 33-37 mgKOH / g;

[0060] 8. White carbon black: Cabot EH-5 fumed white carbon black;

[0061] 9. Kaolin: calcined kaolin 1250 mesh;

[0062] 10. Talc: 1250 mesh, silicon dioxide content 60-70%;

[0063] 11. Vinyl ester resin: Brand: Shangwei, model 977-S;

[0064] 12.POE: Dow, POE 8150.

[0065] Preparation example of modified filler

[0066] Preparation Example 1

[0067] Preparation Example 1 discloses a modified filler, which is prepared by the following steps:

[0068] A1. Add 4 kg of white carbon black as a powder filler to 8 kg of 50 wt% ethanol aqueous solution, then add 0.05 kg of γ-(2,3-epoxypropoxy)propyltrimethoxysilane as a silane coupling agent, heat to 50 ° C for reaction, react for 1 hour, filter, and then dry at 80 ° C for 1 hour to obtain a pretreated powder filler;

[0069] A2. Add 0.1 kg of allyl glycidyl ether to the pretreated powder filler, stir for 20 minutes, add 0.2 kg of vinyl ester resin after stirring evenly, heat to 60°C, knead and stir for 30 minutes to obtain a modified filler.

[0070] Preparation Example 2-3

[0071] The difference between Preparation Example 2-3 and Preparation Example 1 is that the amount of raw materials used and the preparation conditions are different, see Table 1 below for details.

[0072] Table 1 Raw material dosage and preparation conditions of Preparation Examples 1-3

[0073]

[0074]

[0075] Preparation Comparative Example 1

[0076] The difference between Preparation Comparative Example 1 and Preparation Example 1 is that an equal amount of allyl glycidyl ether is replaced by polyethylene glycol 400, and the rest is the same as Preparation Example 1.

[0077] Preparation Comparative Example 2

[0078] The difference between Preparation Comparative Example 2 and Preparation Example 1 is that the vinyl ester resin is replaced by an epoxy resin (commercially available, bisphenol A type liquid epoxy resin E-44) in equal amount, and the rest is the same as Preparation Example 1.

[0079] Preparation Comparative Example 3

[0080] The difference between Preparation Comparative Example 3 and Preparation Example 1 is that an equal amount of allyl glycidyl ether is replaced by vinyl ester resin, and the rest is the same as Preparation Example 1.

[0081] Example

[0082] Example 1

[0083] Embodiment 1 discloses a PCR HIPS material for a POSS machine, which is prepared by the following steps:

[0084] S1. Bake 5 kg of PCR HIPS at 70° C. for 45 min to obtain PCR HIPS processed material;

[0085] S2, adding the above-prepared PCR HIPS processed material, 1.5kg K resin, 0.8kg SEBS as a toughening agent, 0.3kg styrene-octene-glycidyl methacrylate copolymer as a compatibilizer and 0.45kg POE as a stabilizer into a reactor, stirring for 20 minutes, stirring evenly, to obtain a mixture A;

[0086] S3, adding 1.2 kg of commercially available white carbon black as a filler, 0.1 kg of pentaerythritol stearate as a lubricant and 0.05 kg of an antioxidant to the mixture A, wherein the antioxidant is composed of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:1.5, and stirring for 30 min until uniform, to obtain a PCR HIPS mixture;

[0087] S4. Add the PCR HIPS mixture into a twin-screw extruder, adjust the temperature of the twin-screw extruder, set the temperature of zone 1 to 190°C, the temperature of zone 2 to 210°C, the temperature of zone 3 to 220°C, the temperature of zone 4 to 230°C, the temperature of zone 5 to 220°C, the temperature of zone 6 to 210°C, the die temperature to 220°C, the screw speed to 300r / min, and perform water cooling and hot air drying after extrusion, and then pelletize to obtain PCR HIPS material.

[0088] Example 2-3

[0089] The difference between Example 2-3 and Example 1 is that the amount of raw materials used and the preparation conditions are different, see Table 2 below for details.

[0090] Table 2 Raw material dosage and preparation conditions of Examples 1-3

[0091]

[0092]

[0093] Embodiment 4-9

[0094] The difference between Examples 4-9 and Example 1 is that the sources of the fillers are different, see Table 3 for details.

[0095] Table 3 Sources of fillers in Examples 4-9

[0096] Example Source of filler Example 4 Preparation Example 1 Example 5 Preparation Example 2 Example 6 Preparation Example 3 Example 7 Preparation Comparative Example 1 Example 8 Preparation Comparative Example 2 Example 9 Preparation Comparative Example 3

[0097] Example 10

[0098] The difference between Example 10 and Example 4 is that the toughening agent is different. The toughening agent in Example 10 is composed of SEBS, vinyl-terminated polydimethylsiloxane and polyoxypropylene triol in a weight ratio of 1:0.4:0.1, and the rest is the same as Example 4.

[0099] Embodiment 11

[0100] The difference between Example 11 and Example 10 is that the toughening agent is composed of SEBS, vinyl-terminated polydimethylsiloxane and polyoxypropylene triol in a weight ratio of 1.5:0.8:0.3, and the rest is the same as Example 10.

[0101] Example 12

[0102] The difference between Example 12 and Example 10 is that the toughening agent consists of SEBS and hydroxyl-terminated polydimethylsiloxane in a weight ratio of 1:0.5, the average molecular weight of the hydroxyl-terminated polydimethylsiloxane is 1000-2000, the hydroxyl value is 1.6-2mmol / g, and the viscosity is 300-500 (25°C, mpa·s). The rest is the same as Example 10.

[0103] Embodiment 13

[0104] The difference between Example 13 and Example 10 is that the stabilizer is different. The stabilizer in Example 13 is composed of POE and a long-chain alkyl silane coupling agent in a weight ratio of 1:0.2, and the long-chain alkyl silane coupling agent is dodecyltrimethoxysilane. The rest is the same as Example 10.

[0105] Embodiment 14

[0106] The difference between Example 14 and Example 13 is that the stabilizer consists of POE and a long-chain alkyl silane coupling agent in a weight ratio of 1:0.6, and the rest is the same as Example 13.

[0107] Comparative Example

[0108] Comparative Example 1

[0109] The difference between Comparative Example 1 and Example 1 is that the K resin is replaced by an equal amount of polypropylene resin, the polypropylene resin is from Mitsui Chemicals, model TA114, and the melt index is 0.98 g / 10 min. The rest is the same as Example 1.

[0110] Comparative Example 2

[0111] The difference between Comparative Example 2 and Example 1 is that the stabilizer is replaced by a toughening agent in equal amount, and the other components are the same as Example 1.

[0112] Performance Test The PCR HIPS materials prepared in Examples 1-14 and Comparative Examples 1-2 were subjected to performance tests. The PCR HIPS materials prepared above were placed in an oven at 75° C. and baked for 90 min. They were injection molded using an injection molding machine at a temperature of 220° C. and cut into test strips for testing:

[0113] (1) Impact strength test

[0114] According to the test standard of ASTM D256, the above test strip is subjected to the Izod notched impact strength test (unit: J / m), recorded as the first impact strength, and the test result is tested and recorded;

[0115] (2) Scratch resistance test

[0116] Use TABER abrasion tester, load 500g, use standard artificial sweat with pH=6.5 as test solution, take 0.2ml and drop it on the test wheel, set the number of test laps, adjust the speed to 60r / min for testing, observe every 25 laps, and record the number of frictions when the test strip shows wear, scratches or discoloration;

[0117] (3) Aging resistance test

[0118] The above test strips were placed in a constant temperature and humidity chamber, tested for 7 days at a temperature of 85° C. and a humidity of 85%, and then returned to room temperature (25° C.). Referring to the test standard of ASTM D256, the test strips were subjected to a cantilever beam notched impact strength test (unit: J / m), recorded as the second impact strength, and the impact strength change rate (unit: %) was calculated, where the impact strength change rate = (first impact strength - second impact strength) / first impact strength * 100%, and the test results were tested and recorded. The following are the performance test data of the PCR HIPS materials prepared in Examples 1-14 and Comparative Examples 1-2, see Table 4 for details.

[0119] Table 4 Performance test data of Examples 1-14 and Comparative Examples 1-2

[0120]

[0121] It can be seen from Examples 1-3 and 4-9 that by compounding the applied allyl glycidyl ether and vinyl ester resin and modifying the powder filler with a silane coupling agent, the impact strength, scratch resistance and aging resistance of the prepared PCR HIPS material can be improved. When used in POSS machines, it has good drop resistance, scratch resistance and aging resistance, and is not prone to aging and discoloration after long-term use.

[0122] It can be seen from Examples 4-9 and 10-12 that the use of SEBS, vinyl-terminated polydimethylsiloxane and polyoxypropylene triol in a preferred ratio of the present application for compounding and using as a toughening agent can improve the impact strength, scratch resistance and aging resistance of the prepared PCRHIPS material.

[0123] It can be seen from Example 10 and Examples 13-14 that the use of the long-chain alkyl silane coupling agent of the present application and POE in combination can further improve the impact strength, scratch resistance and aging resistance of the prepared PCR HIPS material.

[0124] It can be seen from Example 1 and Comparative Examples 1-2 that the compounding of the filler, K resin, toughening agent and stabilizer of the present application can produce a good synergistic effect, improve the compatibility with PCR HIPS, and is suitable for the formulation system of the present application. The obtained PCR HIPS has good performance in all aspects.

[0125] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A PCR HIPS material for a POSS machine, characterized in that: It is prepared from the following raw materials in parts by weight: PCR HIPS 50-80 copies K resin 15-25 parts Filling 12-22 parts Toughener 4-8 parts 3-8 parts of compatibilizer 1-3 parts lubricant Stabilizer 2.5-4.5 parts 0.5-2 parts of antioxidant; The toughening agent is composed of SEBS, vinyl-terminated polydimethylsiloxane and polyoxypropylene triol in a weight ratio of (1-1.5): (0.4-0.8): (0.1-0.3); The filler is a modified filler, and the modified filler is prepared from the following raw materials in parts by weight: Powder filler 40-60 parts Silane coupling agent 0.5-2 parts Vinyl ester resin 0.5-2 parts 1-3 parts of allyl alcohol glycidyl ether; The powder filler is any one or a combination of white carbon black, kaolin, and talc; the silane coupling agent is any one or a combination of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, vinyltrimethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, and γ-aminopropyltriethoxysilane; The modified filler is prepared by the following steps: A1. Add 40-60 parts of powder filler to 80-120 parts of 50-85wt% ethanol aqueous solution, then add 0.5-2 parts of silane coupling agent, heat to 50-65°C for reaction, react for 1-2h, filter, and dry to obtain pretreated powder filler; A2. Add 1-3 parts of allyl glycidyl ether to the pretreated powder filler, mix well, then add 0.5-2 parts of vinyl ester resin, heat to 60-80°C, knead and stir, stir for 30-60 minutes, to obtain a modified filler; The compatibilizer is any one of styrene-octene-glycidyl methacrylate copolymer and styrene-acrylonitrile-glycidyl methacrylate copolymer; the stabilizer is composed of POE and a long-chain alkyl silane coupling agent in a weight ratio of 1: (0.2-0.6).

2. A PCR HIPS material for a POSS machine according to claim 1, characterized in that, The lubricant is one or more combinations of pentaerythritol stearate, ethylene bis stearamide, zinc stearate, and triphenyl phosphate.

3. A PCR HIPS material for a POSS machine according to claim 1, characterized in that, The antioxidant consists of antioxidant 1010 and antioxidant 168 in a weight ratio of 1:(1.5-2.5).

4. A method for preparing a PCR HIPS material for a POSS machine as described in any one of claims 1 to 3, characterized in that: The method comprises the following preparation steps: S1, baking the PCR HIPS raw material to obtain the PCR HIPS processed material; S2, adding PCR HIPS processing material, K resin, toughening agent, compatibilizer and stabilizer into the reaction equipment, stirring evenly to obtain mixture A; S3, adding filler, lubricant and antioxidant to mixture A, stirring evenly to prepare PCR HIPS mixture; S4, melt-extrude the PCR HIPS mixture, cool, dry and pelletize to obtain the PCR HIPS material.

5. A method for preparing a PCR HIPS material for a POSS machine according to claim 4, characterized in that, The baking temperature in step S1 is 70-80°C, and the baking time is 45-120 minutes; the melting temperature in step S4 is 190-230°C.