Low light transmittance shading film and its processing technology

By using hyperbranched polysiloxane and epoxy resin modified pigments in the light-shielding film to form a cross-linking network, the problem of simultaneously improving the toughness and light-shielding properties of the light-shielding film is solved, and the effects of high light-shielding properties and high toughness are achieved.

CN118165497BActive Publication Date: 2024-11-19KUNSHAN RED APPLE PLASTIC NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410359840.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-11-19
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

When the existing light-shielding film improves light-shielding properties, its toughness decreases, and it is difficult to simultaneously improve the toughness and light-shielding properties of the light-shielding film.

Method used

Hyperbranched polysiloxane is used as a toughening agent, and an epoxy resin organic encapsulation layer is introduced on the surface of the inorganic pigment. The modified pigment forms a cross-linking network with the thermoplastic polyurethane to improve the toughness and light transmittance of the light shielding film.

Benefits of technology

The toughness and light-shielding properties of the light-shielding film are significantly improved, making it have excellent high light-shielding properties and high toughness, uniform light-shielding and consistent light transmittance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004762462030000091
    Figure BDA0004762462030000091
  • Figure BDA0004762462030000101
    Figure BDA0004762462030000101
Patent Text Reader

Abstract

The present application relates to the field of TPU films, and specifically discloses a low-transmittance shading film and its processing technology. The low-transmittance shading film comprises the following components in parts by mass: 100 parts of thermoplastic polyurethane elastomer, 40-60 parts of shading masterbatch, 25-30 parts of matte agent, 10-25 parts of hyperbranched polysiloxane, and 1-4 parts of antioxidant; the shading masterbatch comprises the following components in parts by mass: 20-40 parts of thermoplastic polyurethane elastomer, 60-80 parts of modified pigment, and 1-3 parts of dispersant; the modified pigment is an inorganic pigment grafted with epoxy resin; its preparation method is: according to the ratio, the raw materials are mixed evenly to obtain a mixture; the mixture is extruded, cooled, and pelletized to obtain prefabricated particles; the prefabricated particles are cast and cooled to obtain a low-transmittance shading film. The low-transmittance shading film of the present application has the advantages of better shading and excellent toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of TPU films, and more specifically, to a low-light-transmittance shading film and a processing technology thereof. Background Art

[0002] The shading film can be used to block light, achieving the effect of partial light transmission or complete light blocking, thereby achieving the control of light to meet specific shading needs. The base material of the shading film can be a polymer film such as a polyolefin film, a polyimide film or a polyurethane film. Among them, thermoplastic polyurethane (TPU) is a polymer compound with carbamate as a repeating unit generated by the reaction of polyols and polyisocyanates. It has the characteristics of adjustable hardness, solvent resistance, and low temperature resistance, and has good adhesion to most materials. It is a polymer material with comprehensive properties, so it is widely used in tablecloths, shower curtains, curtains, furniture fabrics, coated fabrics and lining materials.

[0003] The related technology provides a high light-shielding two-color TPU film, including a black film for light-shielding and a white film for heat insulation. The raw materials of the black film include 100 parts of TPU masterbatch and 30-50 parts of silane coupling agent modified carbon black. The carbon black is modified with a silane coupling agent so that the carbon black can be better dispersed in the TPU, thereby achieving an excellent light-shielding effect.

[0004] However, the large amount of inorganic pigments added to the light-shielding film increases the rigidity of the light-shielding film while decreasing its toughness. How to simultaneously improve the toughness and light-shielding properties of the light-shielding film is one of the problems that need to be solved in the current light-shielding film application field. Summary of the invention

[0005] In order to enhance the toughness and light-shielding property of a light-shielding film, the present application provides a low-light-transmittance light-shielding film and a processing technology thereof.

[0006] In a first aspect, the present application provides a low-transmittance shading film, which adopts the following technical solution:

[0007] A low-transmittance shading film comprises the following components in parts by weight:

[0008] 100 parts of thermoplastic polyurethane elastomer,

[0009] 40-60 parts of light-shielding masterbatch,

[0010] 25-30 parts of matte agent,

[0011] Hyperbranched polysiloxane 10-25 parts,

[0012] 1-4 parts of antioxidants;

[0013] The light-shielding masterbatch comprises the following components in parts by mass:

[0014] Thermoplastic polyurethane elastomer 20-40 parts,

[0015] 60-80 parts of modified pigment,

[0016] 1-3 parts of dispersant;

[0017] The modified pigment is an inorganic pigment grafted with epoxy resin.

[0018] By adopting the above technical scheme, hyperbranched polysiloxane is used as a toughening agent. Hyperbranched polysiloxane can significantly coordinate the rigidity and flexibility of the long chain of thermoplastic polyurethane elastomer polymer. The unique branched structure and rich functional end groups of hyperbranched polysiloxane enable it to form a cross-linked network with the long chain of polyurethane to interpenetrate, and can react to form a chain network that is beneficial to absorbing impact energy, thereby enhancing the toughness of the light-shielding film. At the same time, the light-shielding masterbatch is improved in this application, and an epoxy resin organic coating layer is introduced on the surface of the inorganic pigment to improve the compatibility of the inorganic pigment with the polyurethane organic system, promote the uniform dispersion of the inorganic pigment in the light-shielding film, and make the light-shielding film have better low light transmittance. And the hydroxyl-modified epoxy resin It can react with hyperbranched polysiloxane and polyurethane long chains to participate in the formation of a cross-linked interpenetrating network, enrich the flexible chain segments of the polyurethane organic system, and further promote the improvement of the toughness of the light-shielding film. At the same time, since the epoxy resin-modified pigment is connected with the hyperbranched polysiloxane and polyurethane long chains by means of the grafted epoxy resin segments, and the hyperbranched branched structure makes the epoxy resin-modified pigment more effectively distributed in the cross-linked interpenetrating network, and is not easy to form agglomerations in the mixed system, and maintains an excellent dispersion effect in the whole process. The applicant has found that through the above method, the light-shielding property of the film is significantly improved, so that the prepared light-shielding film has uniform light-shielding and consistent light transmittance, and the light-shielding film has excellent high light-shielding property and high toughness.

[0019] Preferably, the hyperbranched polysiloxane is obtained by hydrolysis and co-condensation of an organic siloxane monomer, and the organic siloxane monomer comprises the following components in percentage by mass: 30-50% vinyl siloxane, 20-30% tetraethyl orthosilicate, and 30-40% dialkyldialkoxysilane.

[0020] By adopting the above technical solution, selecting the above polymerization monomers and controlling the mass percentage of the monomers, the obtained hyperbranched polysiloxane can have abundant hydroxyl groups and a suitable degree of branching.

[0021] Preferably, the preparation method of the hyperbranched polysiloxane comprises the following steps:

[0022] The organic siloxane monomer is mixed with water, the pH value is adjusted to 1-3, pre-hydrolyzed at room temperature for 10-20 minutes under an inert atmosphere, reacted at 60-90° C. for 3-8 hours, distilled under reduced pressure, and dried in vacuum to obtain a hyperbranched polysiloxane.

[0023] By adopting the above technical scheme, under acidic catalytic conditions, the silicon-oxygen bond of the organic siloxane monomer is broken to generate a silicon hydroxyl intermediate, which is then condensed to form a silicon-oxygen-silicon bond to generate a hyperbranched polysiloxane containing a certain amount of silicon hydroxyl groups; a certain amount of vinyl siloxane, ethyl orthosilicate, and dimethyldiethoxysilane are used as the reaction raw materials of the hyperbranched siloxane, so that the generated hyperbranched polysiloxane can have a considerable amount of silicon hydroxyl groups and good chemical reaction activity;

[0024] Hyperbranched siloxane has abundant silicon-oxygen-silicon chain segments and good flexibility, and can improve the toughness and wear resistance of the shading film; hyperbranched siloxane has good reactivity, and can form a cross-linked network with long polyurethane chains and long hydroxyl-modified epoxy resin chains on the surface of modified pigments to interpenetrate, further promoting the improvement of the toughness of the shading film; by controlling the percentage of each reactive monomer of the hyperbranched siloxane, the hyperbranched siloxane has abundant hydroxyl groups and a suitable degree of branching, thereby improving the reactivity and toughness of the hyperbranched siloxane and ensuring the toughness of the cross-linked network.

[0025] Preferably, the preparation method of the modified pigment comprises:

[0026] dispersing the epoxy resin in an organic solvent to obtain an epoxy resin dispersion;

[0027] The inorganic pigment, organic solvent and polyisocyanate are mixed, stirred at room temperature for 20-30 minutes under an inert atmosphere, then heated to 30-90°C, and the epoxy resin dispersion is added dropwise. After the addition is completed, the mixture is reacted at 100-200°C for 8-24 hours. After the reaction is completed, the mixture is washed with an organic solvent, filtered and dried to obtain a modified pigment.

[0028] Preferably, the epoxy resin is bisphenol A epoxy resin; and the organic solvent is selected from one of acetone, xylene and toluene.

[0029] Preferably, the mass ratio of the inorganic pigment, polyisocyanate and epoxy resin is 1:(0.4-0.6):(0.5-0.8).

[0030] By adopting the above technical scheme, using polyisocyanate as a bridging agent and grafting epoxy resin onto the surface of inorganic pigment, the compatibility of inorganic pigment and polyurethane organic system can be improved, the uniform distribution of inorganic pigment can be promoted, and the shading effect can be improved; the epoxy resin chain segments can participate in the formation of cross-linked network interpenetration, enrich the flexible chain segments of the polyurethane system, enhance the loading and dispersion of the pigment, and promote further improvement of the toughness and shading property of the shading film.

[0031] Preferably, the inorganic pigment needs to be activated before the grafting modification operation, and the activation treatment step includes:

[0032] The inorganic pigment is dispersed in a hydrogen peroxide solution, subjected to ultrasonic treatment at 80-110° C. for 20-40 minutes, allowed to stand for 4-8 hours, and dried to obtain an activated inorganic pigment.

[0033] By adopting the above technical solution, the surface of the inorganic pigment is endowed with abundant hydroxyl groups, the reaction activity of the inorganic pigment with polyisocyanate is improved, and it is beneficial to improve the grafting rate of the epoxy resin.

[0034] Preferably, the inorganic pigment comprises rutile titanium dioxide and carbon black in a mass ratio of (0.1-0.3):1.

[0035] By adopting the above technical solution, carbon black can provide excellent shading effect, rutile titanium dioxide can reduce infrared transmittance, shield ultraviolet rays, and have good extinction properties. The combination of the two can make the shading film have lower light transmittance and higher shading effect.

[0036] Preferably, the antioxidant comprises a hindered phenol antioxidant and a phosphite antioxidant in a mass ratio of 1:(1-3).

[0037] Preferably, the dispersant is selected from a combination of one or more of stearic acid amide, zinc stearate, magnesium stearate, and N,N-ethylene bisstearamide.

[0038] In a second aspect, the present application provides a processing technology for a low-transmittance light-shielding film, which adopts the following technical solution:

[0039] A processing technology for a low-light-transmittance shading film comprises the following steps:

[0040] According to the proportion, the thermoplastic polyurethane elastomer, the light-shielding masterbatch, the matte agent, the hyperbranched polysiloxane and the antioxidant are uniformly mixed to obtain a mixture;

[0041] The mixed material is extruded, cooled, and pelletized to obtain prefabricated pellets;

[0042] The prefabricated particles are formed by tape casting and cooled to obtain a low-light-transmittance shading film.

[0043] Preferably, the method for preparing the light-shielding masterbatch comprises the following steps:

[0044] Thermoplastic polyurethane elastomer, modified pigment and dispersant are mixed according to the proportion, and then extruded, cooled and pelletized to obtain light-shielding masterbatch.

[0045] By adopting the above technical solution, various raw materials cooperate with each other, so that the prepared light-shielding film has better light-shielding properties and excellent toughness, which promotes the application of the light-shielding film in complex environments.

[0046] In summary, this application has the following beneficial effects:

[0047] 1. Since the present application adopts hyperbranched polysiloxane as a toughening agent, the hyperbranched polysiloxane can significantly coordinate the rigidity and flexibility of the long chain of thermoplastic polyurethane elastomer polymer. The unique branched structure and rich functional end groups of the hyperbranched polysiloxane enable it to form a cross-linked network with the long chain of polyurethane and interpenetrate it, and can react to form a chain network that is conducive to absorbing impact energy, thereby enhancing the toughness of the shading film;

[0048] 2. In the present application, the light-shielding masterbatch is improved by introducing epoxy resin on the surface of inorganic pigment, which improves the compatibility of inorganic pigment with polyurethane organic system, promotes the uniform dispersion of inorganic pigment in the light-shielding film, and makes the light-shielding film have better low light transmittance; and the hydroxyl-modified epoxy resin can react with hyperbranched polysiloxane and polyurethane long chain to participate in the formation of cross-linked interpenetrating network, enriches the flexible chain segment of polyurethane organic system, further promotes the improvement of light-shielding film toughness, and makes the inorganic pigment more effectively distributed in the cross-linked interpenetrating network, has excellent dispersion effect, improves the light-shielding property of the film and makes the light-shielding uniform, so that the light-shielding film has high light-shielding property and high toughness. DETAILED DESCRIPTION

[0049] To further help understand the technical solution of the present invention, the technical solution of the present invention is described in more detail below by providing several specific implementation examples. All of these described embodiments are only partial embodiments of the present invention, not all of them.

[0050] The following specific embodiments may be combined with each other, and the same or similar concepts or processes may not be repeated in some embodiments; and the reaction devices, monomer compounds, antioxidants, and organic solvents involved in the following embodiments are all commercially available.

[0051] The following specific embodiments may be combined with each other, and the same or similar concepts or processes therein may not be described in detail in some embodiments.

[0052] The following examples are further explanations of the present invention, but the present invention is not limited thereto. Unless otherwise specified in the examples, the percentages are all by mass.

[0053] Preparation Example

[0054] Preparation Example 1

[0055] This preparation example provides a hyperbranched polysiloxane, and the preparation method is as follows:

[0056] 4 kg of γ-methacryloxypropyltrimethoxysilane, 2.5 kg of ethyl orthosilicate, 3.5 kg of dimethyldiethoxysilane and 12 kg of water were mixed and stirred evenly, 37 wt % of hydrochloric acid was added dropwise to adjust the pH value to 2, pre-hydrolyzed at room temperature for 15 min in a nitrogen atmosphere, then heated to 65 ° C in a water bath, reacted for 6 h, small molecules were removed by reduced pressure distillation, and vacuum dried to obtain hyperbranched polysiloxane.

[0057] Preparation Example 2

[0058] The only difference between this preparation example and preparation example 1 is that the preparation method of the hyperbranched polysiloxane is as follows:

[0059] 3 kg of γ-methacryloxypropyltrimethoxysilane, 3 kg of ethyl orthosilicate, 4 kg of dimethyldiethoxysilane and 12 kg of water were mixed and stirred evenly, and hydrochloric acid was added dropwise to adjust the pH value to 2. In a nitrogen atmosphere, pre-hydrolysis was carried out at room temperature for 15 minutes, and then heated to 65° C. in a water bath and reacted for 6 hours. Small molecular substances were removed by reduced pressure distillation, and vacuum drying was performed to obtain hyperbranched polysiloxane.

[0060] Preparation Example 3

[0061] The only difference between this preparation example and preparation example 1 is that the preparation method of the hyperbranched polysiloxane is as follows:

[0062] 5 kg of γ-methacryloxypropyltrimethoxysilane, 2 kg of ethyl orthosilicate, 3 kg of dimethyldiethoxysilane and 12 kg of water were mixed and stirred evenly, and hydrochloric acid was added dropwise to adjust the pH value to 2. In a nitrogen atmosphere, pre-hydrolysis was carried out at room temperature for 15 minutes, and then heated to 65° C. in a water bath and reacted for 6 hours. Small molecular substances were removed by reduced pressure distillation, and vacuum drying was performed to obtain hyperbranched polysiloxane.

[0063] Preparation Example 4

[0064] The only difference between this preparation example and preparation example 1 is that the preparation method of the hyperbranched polysiloxane is as follows:

[0065] 4 kg of vinyl triethoxysilane, 2.5 kg of ethyl orthosilicate, 3.5 kg of dimethyldimethoxysilane and 12 kg of water were mixed and stirred evenly. Hydrochloric acid was added dropwise to adjust the pH value to 2. In a nitrogen atmosphere, pre-hydrolysis was carried out at room temperature for 15 minutes, and then heated to 65°C in a water bath and reacted for 6 hours. Small molecules were removed by reduced pressure distillation and vacuum drying was performed to obtain hyperbranched polysiloxane.

[0066] Preparation Example 5

[0067] The only difference between this preparation example and preparation example 1 is that the preparation method of the hyperbranched polysiloxane is as follows:

[0068] 7.5 kg of γ-methacryloxypropyltrimethoxysilane, 2.5 kg of ethyl orthosilicate and 12 kg of water were mixed and stirred evenly. Hydrochloric acid was added dropwise to adjust the pH value to 2. The mixture was pre-hydrolyzed at room temperature for 15 min in a nitrogen atmosphere, and then heated to 65° C. in a water bath and reacted for 6 h. Small molecules were removed by reduced pressure distillation and vacuum drying were performed to obtain hyperbranched polysiloxane.

[0069] Preparation Example 6

[0070] The only difference between this preparation example and preparation example 1 is that the preparation method of the hyperbranched polysiloxane is as follows:

[0071] 6.5 kg of γ-methacryloxypropyltrimethoxysilane, 3.5 kg of dimethyldiethoxysilane and 12 kg of water were mixed and stirred evenly, and hydrochloric acid was added dropwise to adjust the pH value to 2. In a nitrogen atmosphere, pre-hydrolysis was carried out at room temperature for 15 minutes, and then heated to 65° C. in a water bath and reacted for 6 hours. Small molecular substances were removed by reduced pressure distillation, and vacuum drying was performed to obtain hyperbranched polysiloxane.

[0072] Preparation Example 7

[0073] This preparation example provides a modified pigment, and the preparation method is as follows:

[0074] Mix rutile titanium dioxide and carbon black in a mass ratio of 0.2:1 and grind them evenly to obtain a mixed pigment;

[0075] Mix bisphenol A epoxy resin and xylene in a mass ratio of 1:1, stir and disperse evenly to obtain a 50wt% epoxy resin dispersion;

[0076] Take the above 10 kg mixed pigment, mix it with 20 kg acetone and 4.5 kg hexamethylene diisocyanate and place it in a nitrogen atmosphere, stir it at room temperature for 30 minutes, then heat it to 70°C, add 13.6 kg of 50wt% epoxy resin dispersion, and react at 160°C for 12 hours after the addition is completed. After the reaction is completed, wash it three times with acetone, filter it, and vacuum dry it at 65°C to obtain a modified pigment.

[0077] In this preparation example, the model of bisphenol A epoxy resin is WSR 6101 (E44).

[0078] Preparation Example 8

[0079] The only difference between this preparation example and preparation example 7 is that the preparation method of the modified pigment is as follows:

[0080] Take 10 kg of mixed pigment, mix it with 18 kg of acetone and 4 kg of hexamethylene diisocyanate and place it in a nitrogen atmosphere, stir it at room temperature for 30 minutes, then heat it to 70°C, add 10 kg of 50 wt% epoxy resin dispersion, and react at 160°C for 12 hours after the addition is completed. After the reaction is completed, wash it three times with acetone, filter it, and vacuum dry it at 65°C to obtain a modified pigment.

[0081] Preparation Example 9

[0082] The only difference between this preparation example and preparation example 7 is that the preparation method of the modified pigment is as follows:

[0083] Take 10 kg of mixed pigment, mix it with 22 kg of acetone and 6 kg of hexamethylene diisocyanate and place it in a nitrogen atmosphere, stir it at room temperature for 30 minutes, then heat it to 70°C, add 16 kg of 50 wt% epoxy resin dispersion, and react at 160°C for 12 hours after the addition is completed. After the reaction is completed, wash it three times with acetone, filter it, and vacuum dry it at 65°C to obtain a modified pigment.

[0084] Preparation Example 10

[0085] The only difference between this preparation example and preparation example 7 is that the mixed pigment is rutile titanium dioxide and carbon black in a mass ratio of 0.1:1.

[0086] Preparation Example 11

[0087] The only difference between this preparation example and preparation example 7 is that the mixed pigment is rutile titanium dioxide and carbon black in a mass ratio of 0.3:1.

[0088] Preparation Example 12

[0089] The only difference between this preparation example and preparation example 7 is that the preparation method of the modified pigment is as follows:

[0090] Mix rutile titanium dioxide and carbon black in a mass ratio of 0.2:1 and grind them evenly to obtain a mixed pigment;

[0091] Take 10kg of mixed pigment and immerse it in a 35% hydrogen peroxide solution, ultrasonically treat it at 90℃ for 40min, and then let it stand for 6h.

[0092] Filter and dry at 80°C to obtain activated inorganic pigment;

[0093] The above 10 kg activated inorganic pigment was mixed with 20 kg acetone and 4.5 kg hexamethylene diisocyanate and placed in a nitrogen atmosphere, stirred at room temperature for 30 min, then heated to 70°C, and 13.6 kg of 50 wt% epoxy resin dispersion was added dropwise. After the addition was completed, the mixture was reacted at 160°C for 12 h. After the reaction was completed, it was washed three times with acetone, filtered, and dried in vacuo at 65°C to obtain a modified pigment.

[0094] Preparation Example 13

[0095] This preparation example provides a light-shielding masterbatch, including the following components by mass: 3 kg of thermoplastic polyurethane elastomer, 7 kg of modified pigment, and 0.2 kg of dispersant.

[0096] In this preparation example, the model of the thermoplastic polyurethane elastomer is Hexin HY3190AH; the modified pigment is obtained from Preparation Example 7; and the dispersant is zinc stearate.

[0097] The preparation method of light-shielding masterbatch is as follows:

[0098] The thermoplastic polyurethane elastomer, modified pigment and dispersant of the above mass are put into a high-speed mixer and mixed at high speed for 15 minutes; then put into a twin-screw extruder, melt-extrude, pelletize and dry after cooling to obtain a light-shielding masterbatch.

[0099] Preparation Example 14

[0100] The only difference between this preparation example and preparation example 13 is that the light-shielding masterbatch includes the following components in mass: 4 kg of thermoplastic polyurethane elastomer, 6 kg of modified pigment obtained in preparation example 7, and 0.1 kg of dispersant.

[0101] Preparation Example 15

[0102] The only difference between this preparation example and preparation example 13 is that the light-shielding masterbatch includes the following components in mass: 2 kg of thermoplastic polyurethane elastomer, 8 kg of modified pigment obtained in preparation example 7, and 0.3 kg of dispersant.

[0103] Preparation Examples 16-20

[0104] Preparation Examples 16-20 are substantially the same as Preparation Example 11, except that the modified pigments are prepared from Preparation Examples 8-12, respectively.

[0105] Preparation Example 21

[0106] The only difference between this preparation example and preparation example 13 is that the dispersant is stearic acid amide.

[0107] Preparation Example 22

[0108] The only difference between this preparation example and preparation example 13 is that in this preparation example, the preparation method of the modified pigment is as follows:

[0109] Mix rutile titanium dioxide and carbon black in a mass ratio of 0.2:1 and grind them evenly to obtain a mixed pigment;

[0110] 0.2 kg of silane coupling agent KH570 was dispersed in a 95% ethanol aqueous solution adjusted to pH 5 with acetic acid, stirred for 5 minutes, then 10 kg of mixed pigment was added, stirred and heated to 50° C. for reaction for 20 minutes, then filtered, washed and dried to obtain a modified pigment.

[0111] Preparation Example 23

[0112] The only difference between this preparation example and preparation example 13 is that the light-shielding masterbatch includes the following components in mass: 3 kg of thermoplastic polyurethane elastomer, 7 kg of inorganic pigment, and 0.2 kg of dispersant.

[0113] The inorganic pigment is rutile titanium dioxide and carbon black in a mass ratio of 0.2:1.

[0114] The preparation method of light-shielding masterbatch is as follows:

[0115] The thermoplastic polyurethane elastomer, inorganic pigment and dispersant of the above mass are put into a high-speed mixer and mixed at high speed for 15 minutes; then put into a twin-screw extruder, melt-extrude, pelletize and dry after cooling to obtain a light-shielding masterbatch.

[0116] Example

[0117] Example 1

[0118] The present embodiment discloses a low-transmittance shading film, comprising the following components by mass: 10 kg of thermoplastic polyurethane elastomer, 5 kg of shading masterbatch, 2.7 kg of matte agent, 1.8 kg of hyperbranched polysiloxane, and 0.25 kg of antioxidant.

[0119] In this embodiment, the thermoplastic polyurethane elastomer includes 5 kg of Hexin HY3190AH and 5 kg of Bangtai TPU69M85U; the shading masterbatch is prepared by Preparation Example 13; the model of the matte agent is JSR RB810; the hyperbranched polysiloxane is prepared by Preparation Example 1; and the antioxidant includes antioxidant 1010 and antioxidant 168 in a mass ratio of 1:3.

[0120] The processing technology of low light transmittance shading film includes:

[0121] The thermoplastic polyurethane elastomer of the above mass, the light-shielding masterbatch prepared in Preparation Example 13, the matte agent, the hyperbranched polysiloxane prepared in Preparation Example 1, and the antioxidant are put into a high-speed mixer and mixed at high speed for 15 minutes to obtain a mixture;

[0122] The mixed material is put into a twin-screw extruder, melted and extruded, pelletized after cooling, and dried to obtain prefabricated pellets;

[0123] The prefabricated particles are put into a casting machine for extrusion casting, and a low-transmittance light-shielding film is obtained after cooling.

[0124] Example 2

[0125] The only difference between this embodiment and embodiment 1 is that the low-transmittance shading film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 4 kg of shading masterbatch prepared in Preparation Example 13, 2.5 kg of matte agent, 2.5 kg of hyperbranched polysiloxane prepared in Preparation Example 1, and 0.1 kg of antioxidant.

[0126] Example 3

[0127] The only difference between this embodiment and embodiment 1 is that the low-transmittance shading film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 6 kg of shading masterbatch prepared in Preparation Example 13, 3 kg of matte agent, 1 kg of hyperbranched polysiloxane prepared in Preparation Example 1, and 0.4 kg of antioxidant.

[0128] Embodiment 4-8

[0129] Examples 4-8 are substantially the same as Example 1, except that the hyperbranched polysiloxane is prepared by Preparation Examples 2-6.

[0130] Examples 9-16

[0131] Examples 9-16 are substantially the same as Example 1, except that the light-shielding masterbatches are prepared from Preparation Examples 14-21, respectively.

[0132] Comparative Example

[0133] Comparative Example 1

[0134] The only difference between this comparative example and Example 1 is that the low-transmittance light-shielding film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 5 kg of light-shielding masterbatch prepared in Preparation Example 11, 2.7 kg of matte agent, and 0.25 kg of antioxidant.

[0135] The processing technology of low light transmittance shading film includes:

[0136] The thermoplastic polyurethane elastomer of the above mass, the light-shielding masterbatch prepared in Preparation Example 11, the matte agent, and the antioxidant are put into a high-speed mixer and mixed at high speed for 15 minutes to obtain a mixture;

[0137] The mixed material is put into a twin-screw extruder for melt extrusion, pelletized after cooling, and dried to obtain prefabricated particles; the prefabricated particles are put into a casting machine for extrusion casting molding, and a low-transmittance light-shielding film is obtained after cooling.

[0138] Comparative Example 2

[0139] The only difference between this comparative example and Example 1 is that the low-transmittance shading film includes the following components in mass: 10 kg of thermoplastic polyurethane elastomer, 5 kg of shading masterbatch prepared in Preparation Example 11, 2.7 kg of matte agent, 1.8 kg of silane coupling agent (KH570), and 0.25 kg of antioxidant.

[0140] The processing technology of low light transmittance shading film includes:

[0141] The thermoplastic polyurethane elastomer of the above mass, the light-shielding masterbatch prepared in Preparation Example 11, the matte agent, the silane coupling agent, and the antioxidant are put into a high-speed mixer and mixed at high speed for 15 minutes to obtain a mixture;

[0142] The mixed material is put into a twin-screw extruder for melt extrusion, pelletized after cooling, and dried to obtain prefabricated particles; the prefabricated particles are put into a casting machine for extrusion casting molding, and a low-transmittance light-shielding film is obtained after cooling.

[0143] Comparative Example 3

[0144] The only difference between this embodiment and embodiment 1 is that the light-shielding masterbatch is prepared by Preparation Example 22.

[0145] Comparative Example 4

[0146] The only difference between this embodiment and embodiment 1 is that the light-shielding masterbatch is prepared by Preparation Example 23.

[0147] Performance testing

[0148] The low-transmittance shading films prepared in each embodiment and each comparative example were trimmed and cut into shading film samples, and the following tests were performed: Test 1: The tensile strength and elongation at break of the shading film samples of each embodiment and each comparative example were tested with reference to the international standard ASTM-D882-18, the sample film thickness was 0.016 mm, the sample width was 25 mm, the chuck distance was 50 mm, and the test speed was 500 mm / min;

[0149] Test 2: Refer to GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics" to test the notched impact strength of each shading film sample;

[0150] Test 3: Referring to AATCC-148-79 "Evaluation Method for Shading Effect of Curtain Materials", the light transmission "box method" is used to detect the number and average diameter of light-transmitting micropores per square meter of shading film sample, and the grade is evaluated (Grade A is the best).

[0151] The test results are summarized in Table 1

[0152] Table 1

[0153]

[0154]

[0155] It can be seen from Examples 1-3 and Table 1 that the light-shielding film prepared according to the formula and processing technology disclosed in this application has better light-shielding performance, and its tensile strength, notch impact strength and elongation at break are all high, indicating that the light-shielding film of this application has excellent toughness while ensuring the light-shielding effect.

[0156] Combining Example 1, Examples 4-5 and Comparative Examples 1-2 and Table 1, it can be seen that adding hyperbranched polysiloxane as a toughening agent can significantly improve the toughness of the light-shielding film, promote the improvement of tensile strength and notched impact strength, and improve elongation at break. This may be because hyperbranched polysiloxane has abundant flexible silicon-oxygen-silicon segments, which can significantly coordinate the rigid and flexible properties of the thermoplastic polyurethane elastomer polymer long chain, and the unique branched structure and abundant functional end groups of hyperbranched polysiloxane enable it to form a cross-linked network with the polyurethane long chain, and can react to form a chain network that is conducive to absorbing impact energy, thereby enhancing the toughness of the light-shielding film;

[0157] It can be seen from Example 1, Examples 6-8 and Table 1 that the use of vinyl siloxane, tetraethyl orthosilicate and dialkyldialkoxysilane as organic siloxane monomer raw materials to prepare hyperbranched polysiloxane can give the shading film better tensile properties and impact resistance, and promote further improvement of the toughness of the shading film.

[0158] Combining Example 1, Examples 9-12, Comparative Examples 3-4 and Table 1, it can be seen that the use of epoxy resin to modify inorganic pigments can improve the dispersion performance of inorganic pigments, promote the improvement of light-shielding performance, and is conducive to promoting the improvement of tensile properties and impact resistance of the light-shielding film, and enhancing the toughness of the light-shielding film. This may be because the modification of inorganic pigments by epoxy resin can improve the compatibility of inorganic pigments with the polyurethane organic system, promote the uniform distribution of inorganic pigments, and improve the light-shielding effect; and the epoxy resin chain segments can participate in the formation of cross-linked network interpenetration, enrich the flexible segments of the polyurethane system, and promote the further improvement of the toughness of the light-shielding film.

[0159] Combining Example 1, Example 15 and Table 1, it can be seen that the activation treatment of the inorganic pigment before modification can further promote the improvement of the tensile properties and impact resistance of the light-shielding film, and further enhance the toughness of the light-shielding film. This may be because the hydrogen peroxide activation treatment can make the surface of the inorganic pigment have more abundant hydroxyl groups, improve the reactivity of the inorganic pigment with polyisocyanate, and help to increase the grafting rate of the epoxy resin, thereby promoting the further improvement of the toughness of the light-shielding film.

[0160] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low light transmittance shading film, characterized in that: The composition comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer, 40-60 parts of light-shielding masterbatch, 25-30 parts of matte agent, Hyperbranched polysiloxane 10-25 parts, 1-4 parts of antioxidants; The light-shielding masterbatch comprises the following components in parts by mass: Thermoplastic polyurethane elastomer 20-40 parts, 60-80 parts of modified pigment, 1-3 parts of dispersant; The modified pigment is an inorganic pigment grafted with epoxy resin; The hyperbranched polysiloxane is obtained by hydrolysis and co-condensation of an organic siloxane monomer, wherein the organic siloxane monomer comprises the following components in percentage by mass: 30-50% vinyl siloxane, 20-30% tetraethyl orthosilicate, and 30-40% dialkyldialkoxysilane; The preparation method of the modified pigment comprises: dispersing the epoxy resin in an organic solvent to obtain an epoxy resin dispersion; The inorganic pigment, organic solvent and polyisocyanate are mixed, stirred at room temperature for 20-30 minutes under an inert atmosphere, then heated to 30-90° C., and the epoxy resin dispersion is added dropwise. After the addition is completed, the mixture is reacted at 100-200° C. for 8-24 hours. After the reaction is completed, the mixture is washed with an organic solvent, filtered and dried to obtain a modified pigment; The inorganic pigment needs to be activated before the grafting modification operation, and the activation treatment step includes: The inorganic pigment is dispersed in a hydrogen peroxide solution, subjected to ultrasonic treatment at 80-110° C. for 20-40 minutes, allowed to stand for 4-8 hours, and dried to obtain an activated inorganic pigment.

2. The low-light-transmittance shading film according to claim 1, characterized in that: The preparation method of the hyperbranched polysiloxane comprises the following steps: The organic siloxane monomer is mixed with water, the pH value is adjusted to 1-3, pre-hydrolyzed at room temperature for 10-20 minutes under an inert atmosphere, reacted at 60-90° C. for 3-8 hours, distilled under reduced pressure, and dried in vacuum to obtain a hyperbranched polysiloxane.

3. The low-light-transmittance shading film according to claim 1, characterized in that: The inorganic pigment comprises rutile titanium dioxide and carbon black in a mass ratio of (0.1-0.3):

1.

4. The low-light-transmittance shading film according to claim 1, characterized in that: The antioxidant comprises a hindered phenol antioxidant and a phosphite antioxidant in a mass ratio of 1:(1-3).

5. The low-light-transmittance shading film according to claim 1, characterized in that: The dispersant is selected from one or more combinations of stearic acid amide, zinc stearate, magnesium stearate, and N,N-ethylene bisstearamide.

6. A process for processing a low-transmittance light-shielding film according to any one of claims 1 to 5, characterized in that: The following steps are involved: According to the proportion, the thermoplastic polyurethane elastomer, the light-shielding masterbatch, the matte agent, the hyperbranched polysiloxane and the antioxidant are uniformly mixed to obtain a mixture; The mixed material is extruded, cooled, and pelletized to obtain prefabricated pellets; The prefabricated particles are formed by tape casting and cooled to obtain a low-light-transmittance shading film.

7. The processing technology of the low light transmittance shading film according to claim 6, characterized in that: The preparation method of the light-shielding masterbatch comprises the following steps: Thermoplastic polyurethane elastomer, modified pigment and dispersant are mixed according to the proportion, and then extruded, cooled and pelletized to obtain light-shielding masterbatch.