Wear-resistant flame-retardant lubricating coating material and preparation method thereof
By combining modified polyalkyl ketone with graphite and molybdenum disulfide, combined with polyvinyl alcohol modified with 2-carboxyethylphenylphosphinic acid, a wear-resistant and flame-retardant lubricating coating is formed, which solves the problem of bearing resistance in the existing technology. It solves the problems of wear resistance and thermal energy influence, and achieves stable wear resistance and flame retardant performance at high temperatures.
Patent Information
- Application Number
- CN202410477035.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-04-19
AI Technical Summary
When improving the wear resistance and service life of spherical bearings, the existing technology fails to effectively consider the impact of the heat energy generated by friction on the lubricating coating on the bearing surface, and the technical complexity makes it difficult to industrialize.
A wear-resistant and flame-retardant lubricating coating material is used, which is composed of modified polyalkyl ketone, graphite and molybdenum disulfide. A five-membered ring is formed through the reaction of cysteine and polyalkyl ketone to improve the performance of the lubricating coating. Wear resistance and heat resistance, and prepare flame retardants by modifying polyvinyl alcohol with 2-carboxyethylphenylphosphinic acid to form a stable cross-linked carbonized layer to disperse heat.
It achieves the stability and wear resistance of the lubricating coating in high temperature environments, avoids bearing damage caused by frictional heat, and significantly improves the wear resistance and flame retardant properties of the bearings.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment, and in particular to a wear-resistant, flame-retardant, lubricating coating material and a preparation method thereof. Background Art
[0002] Spherical plain bearings are a type of spherical sliding bearings, which are mainly composed of an inner ring with an outer spherical surface and an outer ring with an inner spherical surface. Because the spherical sliding contact surface of spherical plain bearings is large, the inclination angle is large, and most spherical plain bearing parts are processed by special process methods, they have a large load-bearing capacity and impact resistance, and are corrosion-resistant, wear-resistant, self-adjusting, and have good lubrication characteristics. They are widely used. Surface morphology has an important influence on the friction and wear characteristics of spherical plain bearings. In order to reduce friction and wear and extend service life, many scholars have carried out relevant theoretical and experimental research based on the influence of surface texture and solid lubrication on friction characteristics.
[0003] Surface coating technology is a technology that uses a series of processing methods to cover the target material on the surface of the sample to be processed. It has been widely favored in the industrial field in terms of enhancing the anti-wear and friction reduction properties of the surface of parts made of different materials. At present, domestic and foreign researchers have reviewed coating technology and texturing technology, and fully utilized the surface protection of the coating and the lubrication effect of the texture to modify the material. Basnyat et al. (Basnyat P, Luster B, Muratore C, et al. Surface Texturing for Adaptive Solid Lubrication [J]. Surface & Coatings Technology, 2008, 203 (1–2): 73-79.) coated a TiAlCN hard coating on the substrate surface, then used ion etching to texture the TiAlCN surface, and filled MoS2 lubricant on the surface of the textured coating. The friction and wear characteristics were studied at room temperature of 25°C and high temperature of 570°C. The study shows that the textured coating sample can improve the lubrication properties between the friction pairs in two different environments. Xu Shang et al. (Xu Shang, Hua Xijun, Jie Xuan, et al. Research on grease lubrication friction performance of micro-textured surface of TiAlSiN coating on TC11 titanium alloy [J]. New Industrialization, 2018 (3): 27-33.) performed micro-topography on the surface of TC11 titanium alloy, and then coated a layer of TiAlSiN hard coating on the surface, and carried out reciprocating friction test using a friction and wear tester. The study showed that under the conditions of composite lubrication test combining grease lubrication and solid lubrication, the friction pair rotation friction test was carried out, and the TiAlSiN hard coating could play a good protective role on the TC11 titanium alloy substrate. The friction pair surface was relatively intact after the friction test, without obvious wear marks, and the presence of micro-topography could also effectively reduce the friction coefficient.
[0004] Although some current studies have shown that the combination of lubricating coating and texturing technology can optimize the wear resistance and service life of spherical plain bearings, it is still difficult to industrialize due to the complexity of the technology. Moreover, these technologies have not yet considered the impact of heat energy generated by friction on the lubricating coating on the bearing surface. Summary of the invention
[0005] In order to improve the wear resistance and flame retardancy of bearings while simplifying the bearing surface treatment technology, the present invention provides a wear-resistant and flame-retardant lubricating coating material having high compatibility between a flame retardant and a lubricating material and a preparation method thereof.
[0006] A wear-resistant, flame-retardant, lubricating coating material comprises the following components, measured by weight: 8-17 parts of a film-forming agent, 30-38 parts of a lubricant, 1-2 parts of a flame retardant, and 80-100 parts of an organic solvent.
[0007] In some embodiments of the present invention, the method for preparing the film-forming agent comprises the following steps:
[0008] S1: catalytically polymerizing alkenyl ketone under the action of an initiator, the reaction conditions are 70-90°C, the temperature is kept for reaction for 5-7h, the reaction is terminated, and after cooling to room temperature, the reaction is washed with deionized water, the organic layer is collected by stratification, a desiccant is added, and the polyalkyl ketone is obtained by filtration;
[0009] S2: After the polyalkyl ketone obtained in S1 is uniformly mixed with the organic solution containing cysteine, the temperature is maintained at 80-100° C., 0.5-1M alkali solution is added thereto, and after reacting for 2-3 hours, the product is purified by column chromatography to obtain the film-forming agent; the mass ratio of the polyalkyl ketone to cysteine in the reaction system is 2.5-3:1.
[0010] Furthermore, when preparing the film-forming agent, the alkenyl ketone is at least one of methyl vinyl ketone, 1-pentene-3-one, 4-methyl-3-pentene-2-one and phorone.
[0011] Furthermore, when preparing the film-forming agent, the initiator in S1 can be at least one of an organic peroxide initiator, an inorganic peroxide initiator, and an azo initiator, for example, dibenzoyl peroxide, diisopropylbenzene peroxide, potassium persulfate, azobisisobutyronitrile, azobisisoheptylonitrile, etc.
[0012] Furthermore, when preparing the film-forming agent, the desiccant in S2 can be anhydrous sulfate, anhydrous calcium chloride, color-changing silica gel, etc.
[0013] Furthermore, when preparing the film-forming agent, the mass fraction of cysteine in the organic solution containing cysteine is 20-36%; and the solvent used is at least one of N-methylpyrrolidone, N,N-dimethylpropionamide, N-methyl-2-pyrrolidone, and N-ethylpyrrolidone.
[0014] In some embodiments of the present invention, the preparation method of the flame retardant comprises the following steps: dissolving polyvinyl alcohol in an organic solvent 1 under heating conditions, and sequentially adding a catalyst, a dehydrating agent and 2-carboxyethylphenylphosphorous acid, mixing evenly, raising the temperature, reacting for 3-5 hours, cooling to room temperature, adding a ketone organic solvent, continuing to stir evenly, dispersing it in distilled water, and after being evenly dispersed, filtering and drying to obtain the flame retardant.
[0015] Furthermore, when preparing the flame retardant, the molecular weight of the polyvinyl alcohol is 13000-23000, and the polyvinyl alcohol with a product number of 363170 can be purchased from Merck.
[0016] Furthermore, when preparing the flame retardant, the molar ratio of the polyvinyl alcohol to 2-carboxyethylphenyl hypophosphorous acid is 1:59-65.
[0017] Furthermore, when preparing the flame retardant, the organic solvent 1 is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and tetrahydrofuran; the catalyst is at least one of Lewis acids; the dehydrating agent is at least one of anhydrous magnesium sulfate, anhydrous calcium chloride, color-changing silica gel, and anhydrous copper sulfate; and the ketone organic solvent is at least one of acetone, methyl butyl ketone, methyl isobutyl ketone, methyl ethyl ketone, methyl isopropyl ketone, and cyclohexanone.
[0018] In the present invention, the preparation principle of the film-forming agent is to utilize the thiol group in cysteine to react with the ketone group in polyalkyl ketone to form a five-membered ring containing sulfur and nitrogen, and the five-membered ring also carries a carboxyl group. The inventors found through experiments that the formation of the five-membered ring containing S and N can increase the force of the polyalkyl molecular chain, and obtain a modified polyalkyl ketone with good mechanical properties and strong heat resistance. It is used together with graphite and molybdenum disulfide as a component in the lubricating coating, which can improve the wear resistance and heat resistance of the obtained lubricating coating. However, the polyalkyl ketone should not be excessively modified, otherwise the force between the modified polyalkyl ketone molecules will make its hardness too large and unsuitable for use in the lubricating coating.
[0019] The flame retardant is prepared to improve the compatibility of 2-carboxyethylphenyl hypophosphorous acid in the lubricating coating system. Moreover, the introduction of polyethylene carbon chain enables the flame retardant to produce a cross-linked carbonized layer with a more stable structure when heated. The formation of the carbonized layer can disperse heat and enhance the flame retardant and high temperature resistance of the lubricating coating.
[0020] In some embodiments of the present invention, the lubricant is a composition of graphite powder and molybdenum disulfide, and the mixing mass ratio of the two is 1.5-3:1.
[0021] In some embodiments of the present invention, the organic solvent is at least one of an ester solvent and an alcohol solvent, specifically, isopropyl acetate, n-butyl acetate, isopropyl alcohol, and the like.
[0022] The preparation method of the wear-resistant, flame-retardant, lubricating coating material described above comprises the following steps: dispersing the film-forming agent and the lubricant in an organic solvent, adding the flame retardant thereto, mixing them evenly and dispersing them ultrasonically to obtain the wear-resistant, flame-retardant, lubricating coating material for mechanical bearings.
[0023] Beneficial effects: Compared with the prior art, the wear-resistant, flame-retardant and lubricating coating material provided by the present invention has the following advantages:
[0024] The flame retardant obtained by modifying polyvinyl alcohol with 1,2-carboxyethylphenyl hypophosphite not only has better compatibility in the lubricating coating material system, but also can form a stable cross-linked carbonized layer when the lubricating coating material generates heat due to multiple frictions, so as to disperse the heat and avoid damage or bulging caused by friction heat at the active part of the bearing to affect the operation of the machine;
[0025] 2. The film-forming agent molecule prepared by modifying polyalkyl ketone with cysteine has no aldehyde structure, is safe and non-toxic, and has a certain content of hetero-five-membered ring in the molecular structure. The five-membered ring contains S and N, and can synergistically enhance the lubrication and wear resistance of the lubricating coating with the graphite powder and molybdenum disulfide in the lubricating coating material system, and also helps the lubricating coating to achieve stronger wear resistance under greater loads. DETAILED DESCRIPTION
[0026] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0027] The conventional lubricating coating used in the present invention is a molybdenum disulfide coating purchased from Chongqing Zhangte Technology Co., Ltd.; the molybdenum disulfide is a 1250 mesh molybdenum disulfide purchased from Shandong Haoyao New Materials Co., Ltd.; the graphite powder is purchased from Zhengzhou Aoyu Chemical Co., Ltd.; and the remaining reagents and equipment are conventional reagents and equipment in this technical field.
[0028] The following is an exemplary description of the preparation process of the film-forming agent and the flame retardant used in the examples:
[0029] Film former-1
[0030] S1: 140g (2 mol) of methyl vinyl ketone was catalytically polymerized under the action of 0.28g of initiator dibenzoyl peroxide, the reaction condition was 70°C, the temperature was kept for reaction for 5h, the reaction was terminated, and after cooling to room temperature, the mixture was washed with deionized water, the organic layer was collected by stratification, 2g of desiccant anhydrous magnesium sulfate was added, and the polyalkyl ketone was obtained by filtration, and the yield was 48.1%;
[0031] S2: After 67 g of the polyalkyl ketone obtained in S1 and 134 g of N-methylpyrrolidone solution with a cysteine mass fraction of 20% are mixed evenly, 15 ml of 0.5 M NaOH solution is added dropwise thereto while maintaining the temperature at 80°C. After reacting for 2 hours, the product is purified by column chromatography to obtain the film-forming agent-1.
[0032] Film former-2
[0033] S1: 168g (2mol) of 1-penten-3-one was catalytically polymerized under the action of 1.68g of potassium persulfate as an initiator at 80°C for 6h, then the reaction was terminated, cooled to room temperature, washed with deionized water, the organic layer was collected, 2g of anhydrous magnesium sulfate as a desiccant was added, and the polyalkyl ketone was obtained by filtration with a yield of 50.5%;
[0034] S2: After 84 g of the polyalkyl ketone obtained in S1 and 111 g of N, N-dimethylpropionamide solution with a cysteine mass fraction of 28% are mixed evenly, 10 ml of 0.8 M KOH solution is added dropwise thereto while maintaining the temperature at 90°C. After reacting for 2 hours, the product is purified by column chromatography to obtain the film-forming agent-2.
[0035] Film former-3
[0036] S1: 196 g (2 mol) of 4-methyl-3-penten-2-one was catalytically polymerized under the action of 0.98 g of potassium persulfate as an initiator at 90°C for 7 h, then the reaction was terminated, cooled to room temperature, washed with deionized water, the organic layer was collected, 2 g of anhydrous magnesium sulfate as a desiccant was added, and the polyalkyl ketone was obtained by filtration with a yield of 49.7%;
[0037] S2: After 97g of the polyalkyl ketone obtained in S1 and 89g of N-methyl-2-pyrrolidone solution with a cysteine mass fraction of 36% are mixed evenly, 10ml of 1.0M KOH solution is added dropwise thereto while maintaining the temperature at 90°C. After reacting for 3h, the product is purified by column chromatography to obtain the film-forming agent-3.
[0038] Film former-4
[0039] S1: 276 g (2 mol) of phorone was catalytically polymerized under the action of 0.138 g of potassium persulfate as an initiator at 90°C for 7 h, then the reaction was terminated, cooled to room temperature, washed with deionized water, the organic layer was collected, 2 g of anhydrous magnesium sulfate as a desiccant was added, and the polyalkyl ketone was obtained by filtration with a yield of 48.3%;
[0040] S2: After 130 g of the polyalkyl ketone obtained in S1 and 120 g of N-methyl-2-pyrrolidone solution with a cysteine mass fraction of 36% are mixed evenly, 10 ml of 1.0 M KOH solution is added dropwise thereto while maintaining the temperature at 90°C. After reacting for 3 hours, the product is purified by column chromatography to obtain the film-forming agent-4.
[0041] Flame retardant-1
[0042] Under heating conditions, 130 g (0.01 mol) of polyvinyl alcohol was dissolved in 500 ml (550 g) of dimethyl sulfoxide, and 6.8 g of aluminum chloride as a catalyst, 5 g of anhydrous magnesium sulfate as a dehydrating agent and 126.26 g (0.59 mol) of 2-carboxyethylphenylphosphorous acid were added in sequence. After mixing evenly, the temperature was raised to 90°C, and the mixture was reacted for 3 hours. The mixture was cooled to room temperature, acetone was added, and the mixture was stirred evenly. The mixture was then dispersed in distilled water. After being evenly dispersed, the mixture was filtered and dried to obtain the flame retardant-1.
[0043] Flame retardant-2
[0044] Under heating conditions, 200 g (0.01 mol) of polyvinyl alcohol was dissolved in 500 ml (474 g) of N, N-dimethylformamide, and 6.74 g of aluminum chloride as a catalyst, 5 g of anhydrous calcium chloride as a dehydrating agent and 132.68 g (0.62 mol) of 2-carboxyethylphenylphosphorous acid were added in sequence. After mixing evenly, the temperature was raised to 100 ° C. After reacting for 4 hours, the mixture was cooled to room temperature, methyl butanone was added, and the mixture was continued to be stirred evenly. Then, the mixture was dispersed in distilled water. After being evenly dispersed, the mixture was filtered and dried to obtain the flame retardant-2.
[0045] Flame retardant-3
[0046] Under heating conditions, 230g (0.01mol) of polyvinyl alcohol was dissolved in 500ml (445g) of tetrahydrofuran, and 6.75g of aluminum chloride as a catalyst, 5g of anhydrous copper sulfate as a dehydrating agent and 139.1g (0.65mol) of 2-carboxyethylphenylphosphorous acid were added in sequence. After mixing evenly, the temperature was raised to 110°C, and the mixture was reacted for 5h. The mixture was cooled to room temperature, methyl butanone was added, and the mixture was stirred evenly. The mixture was then dispersed in distilled water. After being evenly dispersed, the mixture was filtered and dried to obtain the flame retardant-3.
[0047] Example 1
[0048] After dispersing 8 parts of film-forming agent-1 and 30 parts of lubricant (graphite: molybdenum disulfide = 1.5:1) in 80 parts of isopropyl acetate, 1 part of flame retardant-1 is added thereto, mixed evenly and subjected to ultrasonic dispersion to obtain the wear-resistant flame-retardant lubricating coating for mechanical bearings.
[0049] Example 2
[0050] After dispersing 12 parts of film-forming agent-2 and 34 parts of lubricant (graphite: molybdenum disulfide = 2.5:1) in 90 parts of n-butyl acetate, 1 part of flame retardant-2 is added thereto, mixed evenly and subjected to ultrasonic dispersion to obtain the wear-resistant flame-retardant lubricating coating for mechanical bearings.
[0051] Example 3
[0052] After dispersing 17 parts of film-forming agent-3 and 38 parts of lubricant (graphite: molybdenum disulfide = 3:1) in 100 parts of isopropanol, 1 part of flame retardant-3 is added thereto, mixed evenly and subjected to ultrasonic dispersion to obtain the wear-resistant flame-retardant lubricating coating for mechanical bearings.
[0053] Example 4
[0054] Similar to Example 3, except that the film-forming agent used is Film-Forming Agent-4.
[0055] Example 5
[0056] Similar to Example 3, except that in the lubricant, the ratio of graphite to molybdenum disulfide is 1.5:1.
[0057] Example 6
[0058] Similar to Example 3, except that in the lubricant, the ratio of graphite to molybdenum disulfide is 3.5:1.
[0059] Example 7
[0060] Similar to Example 5, except that in the lubricant, the ratio of graphite to molybdenum disulfide is 1:1.
[0061] Comparative Example 1
[0062] Similar to Example 3, except that polyvinyl butyral is used to replace film-forming agent-3.
[0063] Comparative Example 2
[0064] Similar to Example 3, except that flame retardant-3 is not added.
[0065] Comparative Example 3
[0066] A common lubricating coating material on the market.
[0067] Performance Testing
[0068] The lubricating coating materials obtained in Examples 1-7 and Comparative Examples 1-3 were sprayed back and forth evenly on the surface of the same bearing (specifications: inner diameter 55mm, outer diameter 100mm), the spraying pressure was 0.3-0.4MPa, the distance between the spray gun nozzle and the sample was 100-150mm, and the coating thickness was controlled at 10-15μm. The sprayed sample was dried, sintered at 300℃ for 5min, and cooled in the furnace to complete the surface spraying treatment.
[0069] Friction resistance: The bearings were tested using a Pin-on-Disk friction tester to obtain the corresponding friction coefficient and wear amount (mg);
[0070] Flame retardancy: Burn the bearing with an alcohol lamp for 30 seconds and observe the phenomenon.
[0071] The test results are shown in Table 1:
[0072]
[0073] It can be seen from the results in Table 1 that the lubricating coating provided by the present invention is used for the surface of mechanical bearings and has good wear resistance (the friction coefficient of Examples 1-7 is not greater than 0.27, and the wear loss is less than 7.3). However, the composition of the lubricant contained has a certain influence on its wear resistance: It can be seen from the data of Examples 6-7 that when the mass ratio of graphene and molybdenum disulfide is too high or too low, it will cause an increase in the friction coefficient, thereby affecting the wear resistance of the lubricating coating on the bearing surface.
[0074] The results of Comparative Example 1 show that in the system of the lubricating coating of the present invention, the film-forming agent prepared by the present invention is more applicable than polyvinyl butyral (compared with the bearing obtained in Example 3 and Comparative Example 1, the friction coefficient is lower and the flame retardancy is better), and the film-forming agent prepared by cysteine and alkenyl aldehyde is more environmentally friendly and harmless. By comparing the results of Example 3 with those of Comparative Examples 2-3, it can be seen that the importance of flame retardants and the excellent wear resistance and flame retardancy of the lubricating coating provided by the present invention are compared with conventional lubricating coatings on the market.
Claims
1. A wear-resistant, flame-retardant, lubricating coating material, characterized in that: The composition comprises the following components by weight: 8-17 parts of a film-forming agent, 30-38 parts of a lubricant, 1-2 parts of a flame retardant and 80-100 parts of an organic solvent; and the preparation method of the film-forming agent comprises the following steps: S1: catalytic polymerization of alkenyl ketone under the action of initiator, reaction conditions are 70-90°C, heat preservation reaction for 5-7h, then termination of the reaction, cooling to room temperature, washing with deionized water, collecting the organic layer by layers, adding desiccant, filtering to obtain polyalkyl ketone; S2: after uniformly mixing the polyalkyl ketone obtained in S1 and the organic solution containing cysteine, maintaining the temperature at 80-100° C., adding 0.5-1M alkali solution thereto, reacting for 2-3 hours, and purifying the product by column chromatography to obtain the film-forming agent; the mass ratio of the polyalkyl ketone to cysteine in the reaction system is 2.5-3:1; The alkenyl ketone in S1 is at least one of methyl vinyl ketone, 1-penten-3-one, 4-methyl-3-penten-2-one, and phorone; The preparation method of the flame retardant comprises the following steps: dissolving polyvinyl alcohol in an organic solvent 1 under heating conditions, and sequentially adding a catalyst, a dehydrating agent and 2-carboxyethylphenyl hypophosphorous acid, mixing evenly, raising the temperature, reacting for 3-5 hours, cooling to room temperature, adding a ketone organic solvent, continuing to stir evenly, dispersing it in distilled water, and filtering and drying after being evenly dispersed to obtain the flame retardant; The lubricant is a composition of graphite powder and molybdenum disulfide, and the mixing mass ratio of the two is 1.5-3:
1.
2. The wear-resistant, flame-retardant, lubricating coating material according to claim 1, characterized in that: In the organic solution containing cysteine in S2, the mass fraction of cysteine is 20-36%; the solvent used is at least one of N-methylpyrrolidone, N,N-dimethylpropionamide, N-methyl-2-pyrrolidone, and N-ethylpyrrolidone.
3. The wear-resistant, flame-retardant, lubricating coating material according to claim 1, characterized in that: The molecular weight of the polyvinyl alcohol is 13000-23000.
4. The wear-resistant, flame-retardant, lubricating coating material according to claim 1, characterized in that: The molar ratio of the polyvinyl alcohol to the 2-carboxyethylphenyl hypophosphorous acid is 1:59-65.
5. The wear-resistant, flame-retardant, lubricating coating material according to claim 1, characterized in that: The organic solvent 1 is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and tetrahydrofuran; the catalyst is at least one of Lewis acids; the dehydrating agent is at least one of anhydrous magnesium sulfate, anhydrous calcium chloride, color-changing silica gel, and anhydrous copper sulfate; the ketone organic solvent is at least one of acetone, methyl butyl ketone, methyl isobutyl ketone, methyl ethyl ketone, methyl isopropyl ketone, and cyclohexanone.
6. The method for preparing the wear-resistant, flame-retardant, lubricating coating material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: dispersing a film-forming agent and a lubricant in an organic solvent, adding a flame retardant therein, mixing them uniformly and dispersing them ultrasonically to obtain the wear-resistant flame-retardant lubricating coating material.