A high-density tungsten alloy material and preparation method thereof
Through mechanical ball milling, cold isostatic pressure, liquid phase sintering and hot liquid extrusion, high-density tungsten alloy materials were prepared, which solved the problems of long cycles, high energy consumption and unstable performance in the existing processes, and achieved the High strength, toughness and deformation strengthening, suitable for armor-piercing weapons applications.
Patent Information
- Application Number
- CN202410465992.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-18
AI Technical Summary
The existing high-density tungsten alloy preparation process has long cycles, high energy consumption, high cost and unstable performance, making it difficult to meet the requirements of high performance, especially insufficient plasticity and toughness.
The homogeneous modified mixed powder is prepared by mechanical ball milling, and the cold isostatic pressure and liquid phase sintering are carried out, and the force-transfer lubricating medium cover is combined with graphite powder and low-temperature glass powder are used to make a force-transfer lubricating medium cover, and the thermal static liquid is carried out. Extrusion and heat treatment are performed to form a high-density tungsten alloy material.
It significantly improves the strength and toughness of high-density tungsten alloys, shortens the preparation cycle, reduces production costs, and achieves efficient deformation strengthening and material dimensional accuracy. It is suitable as a core material for armor-piercing weapons.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of metallurgical technology, and in particular to a high-density tungsten alloy material and a preparation method thereof. Background Art
[0002] High-density tungsten alloy is a kind of alloy with tungsten as the matrix material (tungsten content is 80-97%) and appropriate additions of Ni, Cu, Fe, Co, Mo, Cr and other elements. Because it overcomes the brittleness of tungsten and maintains the excellent properties of tungsten such as high melting point, high density and low expansion coefficient, it has been widely used in aerospace, military, civil industry and other industries.
[0003] At present, the preparation of high-density tungsten alloy is mainly through rotary forging after sintering. The deformation of rotary forging is small, and it takes multiple heating and forging to obtain a larger deformation. Not only is the cycle long, energy consumption is high, and the cost is high, but the comprehensive performance is not high and unstable, especially the plasticity and toughness are difficult to meet higher performance requirements. Summary of the invention
[0004] The purpose of the present invention is to provide a high-density tungsten alloy material and a preparation method thereof. The high-density tungsten alloy material prepared by the present invention can maintain high toughness while greatly improving strength, and has a short preparation cycle.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a high-density tungsten alloy material, comprising the following steps:
[0007] The tungsten powder, nickel powder and iron powder are subjected to a first mechanical ball milling to obtain a homogeneous modified mixed powder;
[0008] The homogeneous modified mixed powder is subjected to cold isostatic pressing to obtain a cold pressed blank; the relative density of the cold pressed blank is 75-85%;
[0009] The cold pressed blank is subjected to liquid phase sintering to obtain a sintered blank; the liquid phase sintering temperature is 1475-1530° C., and the holding time is 60-130 min; the relative density of the sintered blank is 97.0-99.9%;
[0010] The graphite powder and the low-temperature glass powder are subjected to a second mechanical ball milling, the obtained composite powder is pressed, and the pressed blank is processed to obtain a force transmission lubricating medium sleeve; the softening point of the low-temperature glass powder is 450-900° C.; the relative density of the force transmission lubricating medium is 70-90%;
[0011] The sintered blank is placed in the force transmission lubricating medium jacket, heated to 400-900° C. and kept warm for 40-70 minutes, and then subjected to hot hydrostatic extrusion to obtain an extruded blank; the extrusion ratio of the hot hydrostatic extrusion is 2.5-5, and the extrusion pressure is 1000-1800 MPa;
[0012] The extruded billet is heat treated to obtain a high-density tungsten alloy material;
[0013] The heat treatment comprises: heating the extruded billet to 800-1100° C. for a first time under a protective atmosphere, keeping the temperature for a first time for 2-4 hours, and then cooling the billet to room temperature in a salt bath for a first time; heating the billet cooled to room temperature to 600-1000° C. for a second time under a protective atmosphere, keeping the temperature for a second time for 2-4 hours, and finally cooling the billet to room temperature for a second time.
[0014] Preferably, the liquid phase sintering is performed under a protective atmosphere.
[0015] Preferably, the mass of the tungsten powder is 90-95% of the total mass of tungsten powder, nickel powder and iron powder; the mass of the nickel powder is 3.5-7% of the total mass of tungsten powder, nickel powder and iron powder; the mass of the iron powder is 1.5-3% of the total mass of tungsten powder, nickel powder and iron powder.
[0016] Preferably, the homogeneous modified mixed powder is formed by refined tungsten powder and nanocrystalline nickel-iron solid solution; the particle size of the refined tungsten powder is 500nm~5μm, and the grain size is 14~100nm; the particle size of the nanocrystalline nickel-iron solid solution is 0.2~2μm, and the grain size is 8~100nm.
[0017] Preferably, the cold isostatic pressing pressure is 200-350 MPa.
[0018] Preferably, the particle size of the graphite powder is 500-1500 nm; the particle size of the low-temperature glass powder is 5-40 μm.
[0019] Preferably, the mass of the graphite powder is 50-80% of the total mass of the graphite powder and the low-temperature glass powder.
[0020] Preferably, the second mechanical ball milling has a rotation speed of 60 to 140 rpm and a time of 20 to 50 h.
[0021] Preferably, the pressing pressure is 400-800 MPa.
[0022] The present invention provides a high-density tungsten alloy material prepared by the preparation method described in the above scheme, with a room temperature tensile strength of ≥1600MPa, an elongation of >10%, and an impact toughness of ≥110J / cm 2 .
[0023] The invention provides a preparation method of a high-density tungsten alloy material, comprising the following steps: subjecting tungsten powder, nickel powder and iron powder to a first mechanical ball milling to obtain a homogeneous modified mixed powder; subjecting the homogeneous modified mixed powder to a cold isostatic pressing to obtain a cold pressed blank; the relative density of the cold pressed blank is 75-85%; subjecting the cold pressed blank to liquid phase sintering to obtain a sintered blank; the relative density of the sintered blank is 97.0-99.9%; subjecting graphite powder and low-temperature glass powder to a second mechanical ball milling to press the obtained composite powder, and processing the pressed blank to obtain a force transmission lubricating medium sheath; the softening point of the low-temperature glass powder is 450-900°C; the relative density of the force transmission lubricating medium is 70~90%; placing the sintered billet in the force transmission lubricating medium sleeve, heating it to 400~900℃ and keeping it warm for 40~70min, and then performing hot hydrostatic extrusion to obtain an extruded billet; the extrusion ratio of the hot hydrostatic extrusion is 2.5~5, and the extrusion pressure is 1000~1800MPa; performing heat treatment on the extruded billet to obtain a high-density tungsten alloy material; the heat treatment comprises: first heating the extruded billet to 800~1100℃ under a protective atmosphere, keeping it warm for 2~4h, and then placing it in a salt bath and cooling it to room temperature; second heating the billet cooled to room temperature to 600~1000℃ under a protective atmosphere, keeping it warm for 2~4h, and then cooling it to room temperature.
[0024] The present invention can obtain a homogeneous modified mixed powder with uniform two-phase distribution by mechanically ball-milling the original powder, and can also effectively inhibit the growth of tungsten particles during subsequent liquid phase sintering. Therefore, it can be sintered for a short time at a relatively low temperature to achieve a higher density, which is beneficial to reduce production costs, simplify the process flow, and reduce pollution and component loss during sintering.
[0025] The present invention adopts low-temperature glass powder and graphite powder as raw materials to prepare a force transmission lubricating medium for hot hydrostatic extrusion, which can form a full mixture in a finer microscopic state. When hot hydrostatic extrusion is performed with the force transmission lubricating medium, the softened molten low-temperature glass can be fully combined with the graphite, and the formed uniform tiny force transmission units are adsorbed in the graphite layer, which can form a more stable hydrostatic pressure force transmission lubricating layer, which can not only effectively reduce the extrusion pressure and improve the extrusion process, realize large plastic deformation strengthening, but also ensure the dimensional accuracy of the extruded material.
[0026] The high-density tungsten alloy material prepared by the present invention has a deformation amount of 80%, a room temperature tensile strength of more than 1600MP, an elongation of more than 10%, and has excellent comprehensive properties. It can be used as a core material for armor-piercing weapons and has good armor-piercing power. DETAILED DESCRIPTION
[0027] The present invention provides a method for preparing a high-density tungsten alloy material, comprising the following steps:
[0028] The tungsten powder, nickel powder and iron powder are subjected to a first mechanical ball milling to obtain a homogeneous modified mixed powder;
[0029] The homogeneous modified mixed powder is subjected to cold isostatic pressing to obtain a cold pressed blank; the relative density of the cold pressed blank is 75-85%;
[0030] The cold pressed blank is subjected to liquid phase sintering to obtain a sintered blank; the liquid phase sintering temperature is 1475-1530° C., and the holding time is 60-130 min; the relative density of the sintered blank is 97.0-99.9%;
[0031] The graphite powder and the low-temperature glass powder are subjected to a second mechanical ball milling, the obtained composite powder is pressed, and the pressed blank is processed to obtain a force transmission lubricating medium sleeve; the softening point of the low-temperature glass powder is 450-900° C.; the relative density of the force transmission lubricating medium is 70-90%;
[0032] The sintered blank is placed in the force transmission lubricating medium jacket, heated to 400-900° C. and kept warm for 40-70 minutes, and then subjected to hot hydrostatic extrusion to obtain an extruded blank; the extrusion ratio of the hot hydrostatic extrusion is 2.5-5, and the extrusion pressure is 1000-1800 MPa;
[0033] The extruded billet is heat treated to obtain a high-density tungsten alloy material;
[0034] The heat treatment comprises: heating the extruded billet to 800-1100° C. for a first time under a protective atmosphere, keeping the temperature for a first time for 2-4 hours, and then cooling the billet to room temperature in a salt bath for a first time; heating the billet cooled to room temperature to 600-1000° C. for a second time under a protective atmosphere, keeping the temperature for a second time for 2-4 hours, and finally cooling the billet to room temperature for a second time.
[0035] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0036] The present invention performs a first mechanical ball milling on tungsten powder, nickel powder and iron powder to obtain a homogeneous modified mixed powder.
[0037] In the present invention, the tungsten powder is preferably reduced tungsten powder, the purity is preferably above 99.9%, the average particle size is preferably 1 to 50 μm, and more preferably 5 to 10 μm; the nickel powder is preferably carbonyl nickel powder, the purity is preferably above 99.5%, the average particle size is preferably 1 to 50 μm, and more preferably 5 to 10 μm; the iron powder is preferably carbonyl iron powder, the purity is preferably above 99.5%, the average particle size is preferably 1 to 50 μm, and more preferably 5 to 10 μm.
[0038] In the present invention, the mass of the tungsten powder is preferably 90-95% of the total mass of tungsten powder, nickel powder and iron powder, more preferably 91-94%, and further preferably 92-93%; the mass of the nickel powder is preferably 3.5-7% of the total mass of tungsten powder, nickel powder and iron powder, more preferably 4-6%, and further preferably 4.5-5.5%; the mass of the iron powder is preferably 1.5-3% of the total mass of tungsten powder, nickel powder and iron powder, more preferably 2-2.5%.
[0039] In the present invention, the rotation speed of the first mechanical ball mill is preferably 200-550rpm, more preferably 250-500rpm, and further preferably 300-400rpm; the time of the first mechanical ball mill is preferably 15-45h, more preferably 20-40h, and further preferably 25-35h; the ball-to-material ratio of the first mechanical ball mill is preferably (5-25):1, more preferably (10-20):1; the first ball milling is preferably carried out under a protective atmosphere; the protective gas providing the protective atmosphere is preferably high-purity argon (purity ≥ 99.99%) or nitrogen. The present invention performs the first mechanical ball milling under a protective atmosphere, which can prevent the powder from being oxidized during the ball milling process. The present invention has no special requirements for the equipment used in the first mechanical ball milling, and any ball milling equipment known in the art can be used, such as a stirring high-energy ball mill. The present invention has no special requirements for the grinding ball material used in the first mechanical ball milling, and any grinding ball material known in the art can be used. In the embodiment of the present invention, GCr15 steel balls with a diameter of 8mm are specifically used.
[0040] In order to prevent excessive sticking of the powder during the first mechanical ball milling process, the present invention preferably adds a process control agent during the first mechanical ball milling process. The process control agent is preferably anhydrous ethanol or zinc stearate; the amount of the process control agent added is preferably 0.5-2% of the total mass of tungsten powder, nickel powder and iron powder. In the present invention, adding an appropriate process control agent can significantly improve the powder extraction rate of mechanical ball milling, and is conducive to uniform mixing of powders and industrial production.
[0041] In the present invention, after the first mechanical ball milling, the tungsten powder is refined, and the nickel powder and the iron powder form a solid solution to obtain a homogeneous modified mixed powder composed of refined tungsten powder and nanocrystalline nickel-iron solid solution. The particle size of the refined tungsten powder is preferably 500nm to 5μm, and the grain size is preferably 14 to 100nm; the particle size of the nanocrystalline nickel-iron solid solution is preferably 0.2 to 2μm, and the grain size is preferably 8 to 100nm.
[0042] In the present invention, the homogeneous alloy powder formed by the refined and evenly distributed tungsten powder modified by mechanical ball milling and the nanocrystalline nickel-iron solid solution can effectively prevent the large-scale diffusion and dissolution of tungsten into the nickel-iron solid solution, thereby avoiding the reduction of the plasticity of the alloy material; at the same time, it can also effectively prevent the tungsten particles from growing during the subsequent liquid phase sintering, so that a higher density can be achieved at a relatively low temperature, thereby improving the mechanical properties of the sintered material and the subsequent deformation-strengthened alloy.
[0043] After obtaining the homogeneous modified mixed powder, the present invention performs cold isostatic pressing on the homogeneous modified mixed powder to obtain a cold pressed blank.
[0044] In the present invention, the pressure of the cold isostatic pressing is preferably 200-350MPa, more preferably 250-300MPa, and further preferably 260-290MPa; the time of the cold isostatic pressing is preferably 20-60s, and more preferably 30-50s. The present invention can obtain a cold-pressed blank with higher density, more uniform density distribution and porosity under this pressure, which is conducive to the liquid phase uniformly filling the pores in the subsequent liquid phase sintering process, thereby not easily causing component segregation. In the present invention, the relative density of the cold-pressed blank is 75-85%, preferably 77-83%, and more preferably 79-81%.
[0045] After obtaining the cold pressed blank, the present invention performs liquid phase sintering on the cold pressed blank to obtain a sintered blank.
[0046] In the present invention, the temperature of the liquid phase sintering is 1475-1530°C, preferably 1490-1510°C; the holding time of the liquid phase sintering is 60-130 minutes, preferably 90-120 minutes; the liquid phase sintering is preferably carried out under a protective atmosphere; the protective atmosphere is preferably a hydrogen atmosphere. In the present invention, when the sintering temperature is lower than the above range or the sintering time is too short, the bonding phase will not infiltrate or infiltrate the tungsten phase poorly, resulting in weak bonding between the two phases, which is easy to become a crack source; and when the sintering temperature is higher than the above range or the sintering time is too long, tungsten grains will aggregate and grow, and the tungsten particles will be uneven in size and the bonding phase will be unevenly distributed in the alloy, which will easily reduce the plasticity and toughness of the alloy.
[0047] In the present invention, the relative density of the sintered blank is 97.0 to 99.9%, preferably 97.5 to 99.5%, and more preferably 98.0 to 99.0%.
[0048] The present invention conducts a second mechanical ball milling on graphite powder and low-temperature glass powder, presses the obtained composite powder, and processes the pressed blank to obtain a force transmission lubricating medium sheath.
[0049] In the present invention, the particle size of the graphite powder is preferably 500 to 1500 nm, more preferably 700 to 1300 nm, and further preferably 900 to 1100 nm; the purity of the graphite powder is preferably above 99.8%.
[0050] In the present invention, the particle size of the low-temperature glass powder is preferably 5 to 40 μm, more preferably 10 to 35 μm, and further preferably 20 to 30 μm; the purity of the low-temperature glass powder is preferably above 99.9%; the softening point of the low-temperature glass powder is 450 to 900°C, preferably 500 to 800°C, and more preferably 600 to 700°C.
[0051] In the present invention, the mass of the graphite powder is preferably 50-80% of the total mass of the graphite powder and the low-temperature glass powder, more preferably 55-75%, and further preferably 60-70%.
[0052] In the present invention, the rotation speed of the second mechanical ball mill is preferably 60 to 140 rpm, more preferably 80 to 120 rpm, and further preferably 90 to 100 rpm. The time of the second mechanical ball mill is preferably 20 to 50 h, more preferably 25 to 45 h, and further preferably 30 to 40 h.
[0053] The present invention adopts low-temperature glass powder and graphite powder as raw materials to prepare a force transmission lubricating medium for hot hydrostatic extrusion, which can form a full mixture in a finer microscopic state. When hot hydrostatic extrusion is performed with the force transmission lubricating medium, the softened molten low-temperature glass can be fully combined with the graphite, and the formed uniform tiny force transmission units are adsorbed in the graphite layer, which can form a more stable hydrostatic pressure force transmission lubricating layer, which can not only effectively reduce the extrusion pressure and improve the extrusion process, realize large plastic deformation strengthening, but also ensure the dimensional accuracy of the extruded material.
[0054] In the present invention, the pressing pressure is preferably 400-800 MPa, more preferably 500-700 MPa, and further preferably 550-650 MPa; the pressing is preferably cold pressing. The present invention has no special requirements for the pressing time, as long as it can be formed, which is generally about 30 seconds.
[0055] The present invention has no special requirements for the processing method, and a processing process well known in the art can be used to obtain a force transmission lubricating medium sleeve of a target shape and size. The present invention has no special requirements for the size of the force transmission lubricating medium sleeve, which can be selected according to actual needs; for example, its outer diameter can be 40 mm, and the wall thickness can be 4 to 10 mm.
[0056] After obtaining the sintered blank and the force transmission lubricating medium sheath, the present invention places the sintered blank in the force transmission lubricating medium sheath, heats it to 400-900° C. and keeps it warm for 40-70 minutes, and then performs hot hydrostatic extrusion to obtain an extruded blank.
[0057] In the present invention, the heating temperature is preferably 500-800°C, more preferably 600-700°C; the holding time is preferably 45-65min, more preferably 50-60min; the rate of heating to the heating temperature is preferably 10-20°C / min, more preferably 12-18°C / min, further preferably 14-16°C / min.
[0058] In the present invention, the extrusion ratio of the hot hydrostatic extrusion is 2.5-5 (corresponding to a deformation of 60-80%), preferably 3-4.5, and more preferably 3.5-4; the extrusion pressure of the hot hydrostatic extrusion is 1000-1800 MPa, preferably 1200-1600 MPa, and more preferably 1300-1500 MPa. In the present invention, when the extrusion ratio exceeds 5, extremely high deformation resistance will be generated on the extrusion die and equipment, and the hot hydrostatic extrusion process cannot be implemented, resulting in failure of the extrusion process; when the extrusion ratio is less than 2.5, due to the small deformation, the extruded material cannot obtain high strength and high toughness.
[0059] Before the hot hydrostatic extrusion, the present invention preferably preheats the die used for the hot hydrostatic extrusion, and the preheating temperature is preferably 350-550°C, more preferably 400-500°C.
[0060] The present invention utilizes hot hydrostatic extrusion, and the deformation can reach up to 80%. The deformation degree of tungsten particles increases, and the deformation strengthening effect is more obvious. At the same time, the organization of the material can form a fibrous distribution in the extrusion direction, which is beneficial to improving the self-sharpening and armor-piercing performance of the material; at the same time, it is not only beneficial to improve the strength of tungsten alloy materials, but also can reduce or eliminate the pores in the sintered material, thereby improving the density of the material, and also maintaining a high plasticity and toughness. In addition, due to the use of the force transmission lubricating medium prepared above, the hot hydrostatic extrusion deformation strengthening lubrication conditions are greatly improved, the deformation strengthening effect of the material under the triaxial compressive stress state is excellent, and the material has a high cost performance, which belongs to an efficient short-process advanced preparation technology, and is particularly suitable for mass production.
[0061] The present invention has no special requirements on the shape and size of the extruded blank, and can be selected according to actual needs. In an embodiment of the present invention, the extruded blank is a rod with a diameter of 20 mm.
[0062] After obtaining the extruded billet, the present invention performs heat treatment on the extruded billet to obtain a high-density tungsten alloy material.
[0063] In the present invention, the heat treatment includes: heating the extruded billet to 800-1100°C for the first time under a protective atmosphere and keeping it for 2-4 hours, then placing it in a salt bath and cooling it to room temperature for the first time; heating the billet cooled to room temperature to 600-1000°C for the second time under a protective atmosphere and keeping it for 2-4 hours, and cooling it to room temperature for the second time; as a further preferred solution, the temperature of the first heating is preferably 900-100°C, and the first keeping time is preferably 3 hours; the temperature of the second heating is preferably 700-900°C, and the second keeping time is preferably 3 hours; the rate of the first heating is preferably 10-30°C / min, more preferably 15-25°C / min; the rate of the second heating is preferably 5-20°C / min, more preferably 10-15°C / min. In the present invention, the protective atmosphere during the heat treatment is preferably a nitrogen atmosphere.
[0064] The present invention has no special requirements for the salt bath, and any salt bath known in the art can be used. The present invention preferably places the billet after the first heat preservation in a salt bath furnace for salt bathing. The present invention cools to room temperature in the salt bath to prevent the extruded billet from cracking due to too fast a temperature drop.
[0065] In the present invention, the second cooling is preferably cooling to room temperature in a salt bath.
[0066] The present invention can control the size and distribution of tungsten grains or subgrains and the morphology, size and distribution of precipitated phases through heat treatment, avoid the precipitation of brittle intermetallic compounds, and inhibit the accumulation of impurity elements on the interface of tungsten and bonding phases to obtain a cleaner phase interface; improve dislocation distribution and configuration, and eliminate or partially eliminate residual stress, which plays an important role in improving the dimensional stability of hot hydrostatic extrusion materials, thereby improving the comprehensive mechanical properties of the product.
[0067] The present invention provides a high-density tungsten alloy material prepared by the preparation method described in the above scheme, characterized in that the room temperature tensile strength is ≥1600MPa, the elongation is >10%, and the impact toughness is ≥110J / cm 2 .
[0068] The high-density tungsten alloy material and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0069] The raw materials used in the following examples are as follows:
[0070] Reduced tungsten powder: purity is 99.9%, average particle size is 5μm;
[0071] Carbonyl nickel powder: purity is 99.5%, average particle size is 5μm;
[0072] Carbonyl iron powder: purity is 99.5%, average particle size is 5μm;
[0073] Graphite powder: purity is 99.8%, average particle size is 1.5μm;
[0074] Low temperature glass powder: purity is 99.9%, average particle size is 10μm.
[0075] Example 1
[0076] (1) Mechanical ball milling modification of raw materials
[0077] Reduced tungsten powder, carbonyl nickel powder and carbonyl iron powder were prepared into mixed powder in a mass ratio of 93:4.9:2.1, and then placed in a high-energy stirring ball mill for mechanical ball milling. High-purity argon gas with a purity of 99.9% was used as the protective gas during ball milling, and 1.5wt% of zinc stearate was added as a process control agent. The grinding ball material was GCr15 steel ball with a diameter of 8mm and a ball-to-material ratio (mass ratio) of 25:1. The ball mill speed was controlled to be 550rpm and the ball milling time was 45h. At this time, a modified homogeneous mixed powder of refined tungsten powder with an average size of submicron and a nickel-based solid solution was obtained, and the powder yield was about 95.6%. The tungsten particles modified by ball milling were significantly refined, and the average size had reached the submicron level, about 500nm. The powder particle size was already in the particle size range of ultrafine particles, and the grain size reached about 14nm. The microstructure of the nickel and iron powders modified by ball milling has not only been refined, but also has completely formed a nanocrystalline nickel-based solid solution with a particle size of about 0.2μm and a grain size of about 8nm.
[0078] (2) Cold isostatic pressing and liquid phase sintering
[0079] The modified homogeneous mixed powder prepared above was placed in a rubber sleeve with a wall thickness of about 4 mm, and then placed in a 200MPa ultra-high pressure chamber for cold isostatic pressing to obtain a cold-pressed billet with a relative density of 75%; subsequently, the cold-pressed billet was placed in a hydrogen protective atmosphere sintering furnace, and liquid phase sintering was carried out at 1475°C for 60 minutes to obtain a sintered billet with a relative density of about 97%. The average size of the tungsten particles in the sintered billet is less than 25 μm, and they are spherically distributed in the binding phase, and the distribution of the binding phase is also relatively uniform.
[0080] After testing, the tensile strength of the sintered blank is 1036MPa, the yield strength is 856MPa, the elongation is 23.0%, and the impact toughness is 152J / cm 2 .
[0081] (3) Hot hydrostatic extrusion
[0082] Graphite powder and low-temperature glass powder with a softening point of 450°C are prepared into a composite powder in a mass ratio of 5:5 and then placed in a ball mill for mechanical mixing. The speed of the mixer is 60rpm and the mixing time is 20h. The mechanically mixed composite powder is placed in a steel mold and cold pressed at a pressure of 400MPa to obtain a block blank with a relative density of 70%. After machining, a sheath-shaped force transmission lubrication medium with an outer diameter of about 40mm and a wall thickness of about 4mm can be prepared.
[0083] The sintered blank prepared above was placed in the force transmission lubricating medium jacket prepared above, heated to 400°C at a heating rate of 10°C / min, kept warm for 40 minutes, and then placed in an extrusion die for hot hydrostatic extrusion, the preheating temperature of the die was about 350°C, the extrusion ratio of hot hydrostatic extrusion was 2.5, and the extrusion force was 1000MPa. After extrusion, a rod with a diameter of 20mm was obtained.
[0084] (4) Heat treatment
[0085] The hot liquid-extruded billet is placed in a protective atmosphere heat treatment device, and then heated to 800°C at a heating rate of 10°C / min, kept warm for 2 hours, and then quickly placed in a salt bath furnace to cool to room temperature; the billet cooled to room temperature is placed in a protective atmosphere heat treatment furnace, and heated to 600°C at a heating rate of 5°C / min, kept warm for 2 hours, and then quickly placed in a salt bath furnace to cool to room temperature to obtain a high-density tungsten alloy rod.
[0086] After testing, the deformation of the high-density tungsten alloy rod prepared above reached 60%, the tensile strength reached 1610MPa, the elongation reached 16%, and the impact toughness reached 126J / cm 2 .
[0087] Note: In the present invention, the tensile test refers to GB / T 228.1-2021 to obtain the tensile strength and elongation data; the impact test refers to GB / T 229-2020 to obtain the impact toughness data.
[0088] Example 2
[0089] (1) Mechanical ball milling modification of raw materials
[0090] Reduced tungsten powder, carbonyl nickel powder and carbonyl iron powder are prepared into a mixed powder in a mass ratio of 93:4.9:2.1, and then placed in a high-energy stirring ball mill for mechanical ball milling. During the ball milling, high-purity argon gas with a purity of 99.9% is used as the protective gas, and 1.5wt% of zinc stearate is added as a process control agent. The grinding ball material is GCr15 steel ball with a diameter of 8mm and a ball-to-material ratio (mass ratio) of 15:1. The ball mill speed is controlled to 350rpm and the ball milling time is 30h. At this time, a homogeneous mixed powder of refined tungsten powder and nickel-based solid solution with an average size of submicron level is obtained, and the powder yield is about 97.2%. The tungsten particles modified by ball milling are significantly refined, and the average size has reached the submicron level, about 1.5μm, and the grain size reaches about 14nm. The nickel and iron powders modified by ball milling have all formed nanocrystalline nickel-based solid solutions, with a particle size of about 1.2 μm and a grain size of about 40 nm.
[0091] (2) Cold isostatic pressing and liquid phase sintering
[0092] The modified homogeneous mixed powder prepared above was placed in a rubber sleeve with a wall thickness of about 4 mm, and then placed in a 290 MPa ultra-high pressure chamber for cold isostatic pressing to obtain a cold-pressed billet with a relative density of 80%; subsequently, the cold-pressed billet was placed in a hydrogen protective atmosphere sintering furnace, and liquid phase sintering was carried out at 1495°C for 95 minutes to obtain a sintered billet with a relative density of about 98.8%. The average size of the tungsten particles in the sintered billet was less than 25 μm, and they were spherically distributed in the binding phase, and the distribution of the binding phase was also relatively uniform.
[0093] After testing, the tensile strength of the sintered blank reached 986MPa, the yield strength reached 821MPa, the elongation reached 23.2%, and the impact toughness reached 156J / cm 2 .
[0094] (3) Hot hydrostatic extrusion
[0095] Graphite powder and low-temperature glass powder with a softening point of 650°C are prepared into a composite powder in a mass ratio of 6:4 and placed in a ball mill for mechanical mixing. The speed of the mixer is 100 rpm and the mixing time is 35 hours. The mechanically mixed composite powder is placed in a steel mold and cold pressed at a pressure of 600 MPa to obtain a block blank with a relative density of 81%. After machining, a sheath-shaped force transmission lubrication medium with an outer diameter of about 40 mm and a wall thickness of about 8 mm can be prepared.
[0096] The sintered blank prepared above was placed in the force transmission lubricating medium jacket prepared above, heated to 650°C at a heating rate of 15°C / min, kept warm for 55 minutes, and then placed in an extrusion die for hot hydrostatic extrusion, the preheating temperature of the die was 450°C, the extrusion ratio of hot hydrostatic extrusion was 4, and the extrusion pressure was 1500MPa. After extrusion, a rod with a diameter of 16mm was obtained.
[0097] (4) Heat treatment
[0098] After placing the hot hydrostatic extruded billet in a protective atmosphere heat treatment device, the billet is heated to 950°C at a heating rate of 20°C / min, kept warm for 3 hours, and then quickly placed in a salt bath furnace to cool to room temperature; the billet cooled to room temperature is placed in a protective atmosphere heat treatment furnace, heated to 800°C at a heating rate of 15°C / min, kept warm for 3 hours, and then quickly placed in a salt bath furnace to cool to room temperature to obtain a high-density tungsten alloy rod.
[0099] After testing, the deformation of the high-density tungsten alloy rod prepared above reached 75%, the tensile strength reached 1620MPa, the elongation reached 13%, and the impact toughness reached 118J / cm 2 .
[0100] Example 3
[0101] (1) Mechanical ball milling modification of raw materials
[0102] After the reduced tungsten powder, carbonyl nickel powder and carbonyl iron powder were prepared into a mixed powder in a mass ratio of 93:4.9:2.1, they were placed in a high-energy stirring ball mill for mechanical ball milling. During the ball milling, high-purity argon gas with a purity of 99.9% was used as the protective gas, and 1.5wt% of zinc stearate was added as a process control agent. The grinding ball material was GCr15 steel ball with a diameter of 8mm, a ball-to-material ratio (mass ratio) of 25:1, and the ball mill speed was controlled to 200rpm, and the ball milling time was 45h. At this time, a homogeneous mixed powder of modified tungsten powder and nickel-based solid solution with an average size of submicron was obtained, and the powder yield was about 98.2%. The grain size of the tungsten modified by ball milling reached about 100nm. The nickel and iron powders modified by ball milling have all formed nanocrystalline nickel-based solid solution, with a particle size of about 2μm and a grain size of about 100nm.
[0103] (2) Cold isostatic pressing and liquid phase sintering
[0104] The modified homogeneous mixed powder prepared above was placed in a rubber sleeve with a wall thickness of about 4 mm, and then placed in a 350MPa ultra-high pressure chamber for cold isostatic pressing to obtain a cold-pressed billet with a relative density of about 85%; subsequently, the cold-pressed billet was placed in a hydrogen protective atmosphere sintering furnace and liquid-phase sintered at 1510°C for 130 minutes to obtain a sintered billet with a relative density of about 99.9%.
[0105] According to the test, the tensile strength of the sintered blank is about 960MPa, the yield strength is about 810MPa, the elongation is 25.2%, and the impact toughness is 160J / cm 2 .
[0106] (3) Hot hydrostatic extrusion
[0107] Graphite powder and low-temperature glass powder with a softening point of 900°C are prepared into a composite powder in a mass ratio of 8:2 and placed in a ball mill for mechanical mixing. The speed of the mixer is 140rpm and the mixing time is 50h. The mechanically mixed composite powder is placed in a steel mold and cold pressed at a pressure of about 800MPa to obtain a block blank with a relative density of about 90%. After machining, a sheath-shaped force transmission lubrication medium with an outer diameter of about 40mm and a wall thickness of about 10mm can be prepared.
[0108] The sintered blank prepared above was placed in the force transmission lubricating medium prepared above, heated to 900°C at a heating rate of 20°C / min, kept warm for 70 minutes, and then placed in an extrusion die for hot hydrostatic extrusion, the preheating temperature of the die was about 550°C, the extrusion ratio of hot hydrostatic extrusion was 5, and the extrusion force was 1800MPa. After extrusion, a rod with a diameter of 8.9mm was obtained.
[0109] (4) Heat treatment
[0110] After placing the hot liquid-extruded billet in a protective atmosphere heat treatment device, the temperature of the liquid-extruded billet is increased to 1100°C at a heating rate of 30°C / min, and after keeping warm for 4 hours, it is quickly placed in a salt bath furnace to cool to room temperature; the billet cooled to room temperature is placed in a protective atmosphere heat treatment furnace, the temperature is increased to 1000°C at a heating rate of 20°C / min, and after keeping warm for 4 hours, it is quickly placed in a salt bath furnace to cool to room temperature.
[0111] After testing, the deformation of the high-density tungsten alloy rod prepared above reached 80%, the tensile strength reached 1620MPa, the elongation reached 13%, and the impact toughness reached 112J / cm 2 .
[0112] Comparative Example 1
[0113] The only difference from Example 2 is that the heat treatment in step (4) is not performed. The deformation of the prepared high-density tungsten alloy rod reaches 75%, the tensile strength reaches 1650MPa, the elongation reaches 9%, and the impact toughness reaches 98J / cm 2 .
[0114] Compared with Example 2, the heat treatment was omitted in Comparative Example 1, and the toughness of the obtained high-density tungsten alloy rod was significantly reduced.
[0115] It can be seen from the above embodiments and comparative examples that the present invention provides a high-density tungsten alloy material and a preparation method thereof, which solves the technical defects of the prior art tungsten alloy material such as coarse microstructure, reduced plasticity when the strength is increased, and limited deformation, tensile strength and elongation of the alloy material.
[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a high-density tungsten alloy material, characterized in that: The following steps are involved: The tungsten powder, nickel powder and iron powder are subjected to a first mechanical ball milling to obtain a homogeneous modified mixed powder; the mass of the tungsten powder is 90-95% of the total mass of the tungsten powder, nickel powder and iron powder; the mass of the nickel powder is 3.5-7% of the total mass of the tungsten powder, nickel powder and iron powder; the mass of the iron powder is 1.5-3% of the total mass of the tungsten powder, nickel powder and iron powder; The homogeneous modified mixed powder is subjected to cold isostatic pressing to obtain a cold pressed blank; the relative density of the cold pressed blank is 75-85%; The cold pressed blank is subjected to liquid phase sintering to obtain a sintered blank; the temperature of the liquid phase sintering is 1475-1530° C., and the holding time is 60-130 min; the relative density of the sintered blank is 97.0-99.9%; The graphite powder and the low-temperature glass powder are subjected to a second mechanical ball milling, the obtained composite powder is pressed, and the pressed blank is processed to obtain a force transmission lubricating medium sleeve; the softening point of the low-temperature glass powder is 450-900°C; the relative density of the force transmission lubricating medium is 70-90%; the particle size of the graphite powder is 500-1500nm; the particle size of the low-temperature glass powder is 5-40μm; the mass of the graphite powder is 50-80% of the total mass of the graphite powder and the low-temperature glass powder; the speed of the second mechanical ball milling is 60-140rpm, the time is 20-50h; the pressing pressure is 400-800MPa; The sintered blank is placed in the force transmission lubricating medium jacket, heated to 400-900° C. and kept warm for 40-70 minutes, and then subjected to hot hydrostatic extrusion to obtain an extruded blank; the extrusion ratio of the hot hydrostatic extrusion is 2.5-5, and the extrusion pressure is 1000-1800 MPa; heat treating the extruded billet to obtain a high-density tungsten alloy material; The heat treatment comprises: heating the extruded billet to 900-1100° C. for a first time under a protective atmosphere, keeping the temperature for a first time for 2-4 hours, and then cooling the billet to room temperature in a salt bath for a first time; heating the billet cooled to room temperature to 600-800° C. for a second time under a protective atmosphere, keeping the temperature for a second time for 2-4 hours, and finally cooling the billet to room temperature for a second time.
2. The preparation method according to claim 1, characterized in that: The liquid phase sintering is performed under a protective atmosphere.
3. The preparation method according to claim 1, characterized in that: The homogeneous modified mixed powder is formed by refined tungsten powder and nanocrystalline nickel-iron solid solution; the particle size of the refined tungsten powder is 500nm~5μm, and the grain size is 14~100nm; the particle size of the nanocrystalline nickel-iron solid solution is 0.2~2μm, and the grain size is 8~100nm.
4. The preparation method according to claim 1, characterized in that: The cold isostatic pressing pressure is 200-350 MPa.
5. The high-density tungsten alloy material prepared by the preparation method according to any one of claims 1 to 4, characterized in that: Room temperature tensile strength ≥1600MPa, elongation>10%, impact toughness ≥110J / cm 2 .
Citation Information
Patent Citations
High specific gravity tungsten alloy material and preparation method thereof
CN101386947A
High specific gravity tungsten alloy material and preparation method thereof
CN104313377A
Tungsten-base alloy material and preparation method thereof
CN110358941A
Preparation method of rare earth oxide nano-particle tungsten-nickel-iron alloy with high dispersity and obdurability
CN117107101A
Manufacture of tungsten sintered alloy
JP1990122026A