A kind of ferric phosphate with low sulfur and high iron-phosphorus ratio and its preparation method and application

By performing two slurry and pH adjustment in the preparation process of iron phosphate, the problems of high sulfur content and low iron-phosphorus ratio in the prior art were solved, and iron phosphate with high iron-phosphorus ratio and large specific surface area were obtained, which improved the Electrochemical properties and secondary battery performance.

CN118183658BActive Publication Date: 2024-12-03HUBEI HONGRUN HIGH-TECH NEW MATERIALS CO LTD

Patent Information

Application Number
CN202410354078.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-12-03
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

In the existing iron phosphate preparation methods, the problems of high sulfur content, low iron-phosphorus ratio and small specific surface area lead to low product purity and poor electrochemical performance.

Method used

By performing the first slurry before aging, performing the second slurry after aging, and adding a pH adjuster during the second slurry, the pH value of the first slurry is controlled to avoid generation The by-product of alkaline ammonium ferric phosphate and iron hydroxide improves particle distribution uniformity and reaction area, reduces sulfur content and increases the iron-phosphorus ratio.

Benefits of technology

Iron phosphate with a large specific surface area, low sulfur content and high iron-phosphorus ratio were obtained, which improved the electrochemical performance of its material for preparing lithium iron phosphate as a precursor, and thus improved the electrochemical performance of the positive electrode sheet and the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118183658B_ABST
    Figure CN118183658B_ABST
Patent Text Reader

Abstract

The present application provides a low-sulfur and high-iron-phosphorus iron phosphate and its preparation method and application, belonging to the field of battery material technology. The preparation method of the low-sulfur and high-iron-phosphorus iron phosphate includes: providing amorphous iron phosphate; adding water and phosphoric acid to the amorphous iron phosphate for slurry treatment, and then heating and aging to obtain an aged slurry; slurry washing and filter pressing the aged slurry to obtain a first filter cake; adding water and a first pH regulator to the first filter cake for slurry washing to obtain a first slurry with a pH range of 3.0 to 5.0, and filter pressing the first slurry to obtain a second filter cake; rinsing, drying and calcining the second filter cake to obtain low-sulfur and high-iron-phosphorus iron phosphate. The present application is conducive to the preparation of iron phosphate with low sulfur content, high iron-phosphorus ratio and large specific surface area. The iron phosphate can be used to prepare lithium iron phosphate with better electrochemical performance, and the lithium iron phosphate can be further used to prepare positive electrode plates and secondary batteries with better electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to low-sulfur and high-iron-phosphorus ratio iron phosphate and a preparation method and application thereof. Background Art

[0002] As an important precursor of lithium iron phosphate, the sulfur content, specific surface area, morphology and iron-phosphorus ratio of iron phosphate will affect the performance of lithium iron phosphate. At present, the preparation method of iron phosphate is to first prepare amorphous iron phosphate, and then add excess phosphoric acid for high-temperature aging to complete the crystal transformation to obtain iron phosphate. However, in the case of excessive phosphoric acid, acid salt byproducts such as hydrogen ferric phosphate, dihydrogen ferric phosphate, and ammonium ferric sulfate are easily generated, resulting in low product purity and low iron-phosphorus ratio. At the same time, during the aging process of the above method, the material is easy to agglomerate, the particle distribution is wide, and the excessive surface energy will also cause a large amount of material agglomeration in the subsequent drying and calcination process, resulting in a small specific surface area of ​​the prepared iron phosphate.

[0003] Therefore, the iron phosphate prepared by the existing iron phosphate preparation method has the problems of high sulfur content, low iron-phosphorus ratio and small specific surface area.

[0004] In view of this, this application is hereby filed. Summary of the invention

[0005] In view of the technical problems existing in the background technology, the present application provides a low-sulfur and high-iron-phosphorus ratio ferric phosphate and its preparation method and application, aiming to improve or solve the technical problems mentioned in the background technology.

[0006] In a first aspect, the present invention provides a method for preparing low-sulfur and high-iron-phosphorus iron phosphate, which comprises:

[0007] Providing amorphous iron phosphate;

[0008] The amorphous iron phosphate is slurried by adding water and phosphoric acid, and then aged by heating to obtain an aged slurry;

[0009] The aged slurry is subjected to slurry washing and pressure filtering to obtain a first filter cake;

[0010] Adding water and a first pH adjuster to the first filter cake for slurry washing to obtain a first slurry with a pH value ranging from 3.0 to 5.0, and then filtering the first slurry to obtain a second filter cake;

[0011] The second filter cake is rinsed, dried and calcined to prepare iron phosphate with low sulfur and high iron-phosphorus ratio.

[0012] In the technical solution of the embodiment of the present application, by adding water to the amorphous ferric phosphate for slurry treatment (first slurrying) before aging the crystals, and then after the aging crystal transformation is completed, the first filter cake is slurried again with water (second slurrying), and the first pH regulator is added during or after the second slurrying, it is possible to avoid the first pH regulator being added under the aging high temperature state so that the material undergoes a phase transformation to generate basic ammonium ferric phosphate, thereby helping to reduce the surface energy of the particles, making it difficult for the particles to agglomerate during the subsequent drying and calcining process. Further, in the present application, by controlling the pH value of the first slurry to 3.0 to 5.0, it is possible to avoid the pH value being too high to cause the ferric phosphate to hydrolyze to produce iron hydroxide byproducts, and it is also possible to avoid an excessively high iron-phosphorus ratio.

[0013] Secondly, in the technical solution of the embodiment of the present application, the above two slurrying processes can play a dispersing role, thereby making the overall distribution of the particles more uniform and finer, which is conducive to increasing the reaction area between the particles and the first pH regulator, reducing the generation of acid salts, improving the purity and iron-phosphorus ratio of iron phosphate, and reducing the sulfur content of iron phosphate. Therefore, the preparation method provided by the present application can obtain anhydrous iron phosphate with a large specific surface area, a low sulfur content, and a high iron-phosphorus ratio.

[0014] In some embodiments, the amorphous iron phosphate is slurried by adding water and phosphoric acid, and then the temperature is raised and aged to obtain an aged slurry, comprising:

[0015] Adding water and phosphoric acid to amorphous iron phosphate for slurry treatment to obtain an initial slurry;

[0016] The initial slurry is heated to 80°C to 100°C, and after the initial slurry changes color, the temperature is kept for 60min to 100min to obtain an aged slurry;

[0017] The P / Fe molar ratio of the added phosphoric acid to the amorphous iron phosphate is 0.2:1 to 0.3:1.

[0018] In this embodiment, the aging temperature is controlled at 80°C to 100°C, and after the initial slurry changes color, the heat preservation treatment is continued for 60min to 100min while maintaining the aging temperature at 80°C to 100°C, so that the amorphous iron phosphate can fully undergo crystal transformation. Among them, by setting the P / Fe molar ratio of phosphoric acid to amorphous iron phosphate to 0.2:1 to 0.3:1, the problem of low product purity and low iron-phosphorus ratio caused by acid salt byproducts such as hydrogen ferric phosphate, dihydrogen ferric phosphate, and ammonium ferric sulfate produced under the condition of excessive phosphoric acid can be avoided.

[0019] In some embodiments, the step of adding water and phosphoric acid to amorphous ferric phosphate for slurry treatment to obtain an initial slurry includes:

[0020] The amorphous ferric phosphate is slurried by adding water to obtain a slurry with a solid content of 15% to 30%;

[0021] Under stirring conditions, phosphoric acid is added into a slurry with a solid content of 15% to 30% to obtain an initial slurry.

[0022] In this embodiment, by adding phosphoric acid to the slurry with a solid content of 15% to 30%, it is beneficial to obtain a better dispersion effect in the first slurrying process, specifically, the dispersion degree and dispersion uniformity of the crystals can be improved.

[0023] In some embodiments, a method for preparing amorphous iron phosphate is provided, comprising:

[0024] Dissolving the titanium dioxide byproduct in water to obtain a mixed slurry;

[0025] Adding a second pH adjuster to the mixed slurry to adjust the pH value of the mixed slurry to 4.0-5.0, and then performing solid-liquid separation to obtain a ferrous sulfate solution;

[0026] Mixing ferrous sulfate solution, phosphate solution and hydrogen peroxide to obtain primary amorphous iron phosphate;

[0027] The primary amorphous iron phosphate is rinsed until the conductivity of the rinsing liquid is less than or equal to 5 ms / cm to obtain amorphous iron phosphate.

[0028] In this embodiment, the amorphous iron phosphate prepared by the above method has high purity and stability, which is conducive to obtaining crystals with relatively uniform size and quality during the aging process.

[0029] In some embodiments, the molar ratio of phosphorus in the phosphate solution to iron in the ferrous sulfate solution is 1:1 to 1.1:1; and / or the molar ratio of hydrogen peroxide in the hydrogen peroxide to iron in the ferrous sulfate solution is 0.5:1 to 1:1.

[0030] In this embodiment, by controlling the amount of phosphate solution, hydrogen peroxide and ferrous sulfate solution, on the one hand, it is beneficial to avoid excessive phosphorus reacting with impurities in ferrous sulfate to generate phosphate by-products; on the other hand, it is beneficial to control the pH value of the synthesis process within a more appropriate range, thereby helping to reduce the impurity content in amorphous ferric phosphate and making the particle size of the obtained amorphous ferric phosphate more consistent.

[0031] In some embodiments, the solute in the phosphate solution is selected from at least one of ammonium dihydrogen phosphate and diammonium hydrogen phosphate; and / or, the first pH adjuster is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, sodium hydroxide and ammonia water; and / or, the second pH adjuster is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, sodium hydroxide and ammonia water.

[0032] In this embodiment, the raw materials of the phosphate solution, the first pH adjuster and the second pH adjuster are easily available and relatively cheap, which is beneficial to reducing the production cost of iron phosphate.

[0033] In some embodiments, the second filter cake is rinsed multiple times until the conductivity of the rinsing liquid is less than or equal to 350 us / cm, and then the second filter cake is dried and calcined to prepare iron phosphate with low sulfur and high iron-phosphorus ratio.

[0034] In this embodiment, by controlling the conductivity of the second filter cake to be less than or equal to 350 us / cm, a rinsed second filter cake can be obtained, which is beneficial for obtaining a finished iron phosphate product with higher purity and better consistency.

[0035] In a second aspect, the embodiments of the present application provide a low-sulfur and high-iron-phosphorus ratio iron phosphate, which is prepared by the above-mentioned preparation method of iron phosphate;

[0036] The iron-phosphorus ratio of the low-sulfur and high-iron-phosphorus iron phosphate is 0.977-0.991; and / or, the sulfur content of the low-sulfur and high-iron-phosphorus iron phosphate is 18.55ppm-32.46ppm; and / or, the specific surface area of ​​the low-sulfur and high-iron-phosphorus iron phosphate is 10.50m 2 / g~12.01m 2 / g.

[0037] In the technical scheme of the embodiment of the present application, amorphous iron phosphate is provided; water and phosphoric acid are added to the amorphous iron phosphate for slurry treatment, and then the temperature is raised for aging to obtain an aged slurry; the aged slurry is slurried and washed and filtered to obtain a first filter cake; water and a first pH regulator are added to the first filter cake for slurry washing to obtain a first slurry with a pH value range of 3.0 to 5.0, and then the first slurry is filtered to obtain a second filter cake; the second filter cake is rinsed, dried and calcined. The iron-phosphorus ratio prepared by the method is 0.977 to 0.991, the sulfur content is 18.55 ppm to 32.46 ppm, and the specific surface area is 10.50 m 2 / g~12.01m 2 / g.

[0038] Therefore, the iron phosphate prepared in the present application can overcome the technical problems existing in the prior art and has better electrochemical performance.

[0039] In a third aspect, an embodiment of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode active layer arranged on at least one side of the positive electrode collector, and the positive electrode active layer includes a lithium iron phosphate material prepared using the above-mentioned low-sulfur and high iron-phosphorus ratio iron phosphate as a precursor.

[0040] In this embodiment, the positive electrode plate includes a lithium iron phosphate material prepared using the above-mentioned low-sulfur and high iron-phosphorus ratio iron phosphate as a precursor. The lithium iron phosphate material can inherit the characteristics of the above-mentioned iron phosphate such as low sulfur and high iron-phosphorus ratio, which is conducive to obtaining better electrochemical properties. Therefore, the positive electrode plate including the lithium iron phosphate material also has the advantage of excellent electrochemical properties.

[0041] In a fourth aspect, an embodiment of the present application provides a secondary battery comprising the above-mentioned positive electrode plate.

[0042] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantage of excellent electrochemical performance.

[0043] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0045] Figure 1 The XRD diagrams of the ferric phosphate dihydrate obtained in step (8) of Example 1 of the present application and the ferric phosphate dihydrate obtained in step (5) of Comparative Example 1;

[0046] Figure 2 This is a scanning electron microscope test result diagram of the anhydrous ferric phosphate obtained in step (9) of Example 1 of the present application;

[0047] Figure 3 This is a scanning electron microscope test result diagram of the anhydrous ferric phosphate obtained in step (6) of comparative example 3 of the present application. DETAILED DESCRIPTION

[0048] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0049] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0050] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0051] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0052] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0053] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0054] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0055] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0056] In the prior art, sulfur content, iron-phosphorus ratio, specific surface area and morphology are all important performance indicators of iron phosphate. Among them, the iron-phosphorus ratio of iron phosphate is usually 0.95-0.97, the sulfur content is usually 100ppm-500ppm, and the specific surface area is usually less than 10m 2 / g. At present, the preparation method of iron phosphate is to prepare amorphous iron phosphate first, and then add excess phosphoric acid for high-temperature aging to complete crystal transformation to obtain iron phosphate. However, in the case of excessive phosphoric acid, acid salt byproducts such as hydrogen ferric phosphate, dihydrogen ferric phosphate, and ammonium ferric sulfate are easily generated, resulting in problems such as low product purity and low iron-phosphorus ratio. At the same time, during the aging process of the above method, the material is easy to agglomerate, the particle distribution is wide, and the excessive surface energy will also cause a large amount of material agglomeration in the subsequent drying and calcining process, resulting in a small specific surface area of ​​the prepared iron phosphate.

[0057] In order to solve the technical problems of high sulfur content, low iron-phosphorus ratio and small specific surface area in the prior art iron phosphate, the present application provides a low-sulfur and high iron-phosphorus ratio iron phosphate and a preparation method and application thereof, wherein, by adopting the specific preparation method provided by the present application, including a first slurrying before aging, a second slurrying after aging, and adding a first pH regulator during or after the second slurrying, and controlling the pH value of the first slurry at 3.0-5.0, iron phosphate with a higher iron-phosphorus ratio, lower sulfur content and larger specific surface area can be prepared, thereby improving the electrochemical performance of the lithium iron phosphate material prepared using it as a precursor, and thereby the electrochemical performance of the positive electrode sheet and the secondary battery is also improved.

[0058] The solution of this application is further described below.

[0059] In a first aspect, the present invention provides a method for preparing low-sulfur and high-iron-phosphorus iron phosphate, which comprises:

[0060] Providing amorphous iron phosphate;

[0061] The amorphous iron phosphate is slurried by adding water and phosphoric acid, and then aged by heating to obtain an aged slurry;

[0062] The aged slurry is subjected to slurry washing and pressure filtering to obtain a first filter cake;

[0063] Adding water and a first pH adjuster to the first filter cake for slurry washing to obtain a first slurry with a pH value ranging from 3.0 to 5.0, and then filtering the first slurry to obtain a second filter cake;

[0064] The second filter cake is rinsed, dried and calcined to prepare iron phosphate with low sulfur and high iron-phosphorus ratio.

[0065] In the technical solution of the embodiment of the present application, by adding water to the amorphous ferric phosphate for slurry treatment (first slurry treatment) before aging the crystals, and then after the aging crystal transformation is completed, the first filter cake is slurried again with water (second slurry treatment), and the first pH regulator is added during or after the second slurry treatment, it is possible to avoid the first pH regulator being added under the aging high temperature state so that the material undergoes a phase transformation to generate basic ammonium ferric phosphate (the above-mentioned basic ammonium ferric phosphate is prone to produce ammonia smell during the sintering process), which is beneficial to reducing the surface energy of the particles and making the particles less likely to agglomerate during the subsequent drying and calcining process. By controlling the pH value of the first slurry to 3.0-5.0, it is possible to avoid the pH value being too high to cause the hydrolysis of ferric phosphate to produce iron hydroxide byproducts, and it is beneficial to avoid an excessively high iron-phosphorus ratio.

[0066] Secondly, in the technical solution of the embodiment of the present application, the above two slurrying processes can play a dispersing role, thereby making the overall distribution of the particles more uniform and finer, which is conducive to increasing the reaction area between the particles and the first pH regulator, reducing the generation of acid salts, improving the purity and iron-phosphorus ratio of iron phosphate, and reducing the sulfur content of iron phosphate. Therefore, the preparation method provided by the present application can obtain anhydrous iron phosphate with a large specific surface area, a low sulfur content, and a high iron-phosphorus ratio.

[0067] In some embodiments, a method for preparing amorphous iron phosphate is provided, comprising:

[0068] Dissolving the titanium dioxide byproduct in water to obtain a mixed slurry;

[0069] Adding a second pH adjuster to the mixed slurry to adjust the pH value of the mixed slurry to 4.0-5.0, and then performing solid-liquid separation to obtain a ferrous sulfate solution;

[0070] Mixing ferrous sulfate solution, phosphate solution and hydrogen peroxide to obtain primary amorphous iron phosphate;

[0071] The primary amorphous iron phosphate is rinsed until the conductivity of the rinsing liquid is less than or equal to 5 ms / cm to obtain amorphous iron phosphate.

[0072] In this embodiment, the amorphous ferric phosphate prepared by the above method has high purity and stability, which is beneficial to the subsequent preparation of anhydrous ferric phosphate.

[0073] In some embodiments, the titanium dioxide byproduct includes ferrous sulfate. 2+ The titanium dioxide byproduct is mixed with water at a molar concentration of 1 mol / L to 5 mol / L in the mixed slurry.

[0074] In some embodiments, the second pH adjuster is illustratively but not limitatively selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, sodium hydroxide and ammonia water. Using the above substances as the second pH adjuster has the advantages of easy availability of raw materials and relatively low prices, which is conducive to reducing the production cost of ferric phosphate.

[0075] In some embodiments, the mixed slurry after adjusting the pH value to 4.0-5.0 can be subjected to solid-liquid separation by means of filter press filtration, and the filtrate obtained by separation is allowed to stand for clarification to obtain a ferrous sulfate solution. Exemplarily, the mixed slurry after adjusting the pH value to 5.0 can be subjected to solid-liquid separation by means of filter press filtration.

[0076] In some embodiments, the preparation process of primary amorphous iron phosphate may include: simultaneously dropping a phosphate solution and hydrogen peroxide into a ferrous sulfate solution, and continuing the reaction after the dropping is completed to obtain primary amorphous iron phosphate.

[0077] For example, the molar ratio of phosphorus in the phosphate solution to iron in the ferrous sulfate solution can be 1:1 to 1.1:1, such as 1:1, 1.05:1 or 1.1:1, or any other value in the range of 1:1 to 1.1:1. The molar ratio of hydrogen peroxide in hydrogen peroxide to iron in the ferrous sulfate solution can be 0.5:1 to 1:1, such as 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1 or 1:1, or any other value in the range of 0.5:1 to 1:1.

[0078] By controlling the amount of phosphate solution, hydrogen peroxide and ferrous sulfate solution, on the one hand, it is beneficial to avoid excessive phosphorus from reacting with impurities in ferrous sulfate to form phosphate by-products; on the other hand, it is beneficial to control the pH value of the synthesis process within a more appropriate range, thereby reducing the impurity content in amorphous ferric phosphate and making the particle size of the obtained amorphous ferric phosphate more consistent.

[0079] In some embodiments, the solute in the phosphate solution is illustratively but not limitatively selected from at least one of diammonium phosphate and diammonium hydrogen phosphate. Using the above substances as the solutes of the phosphate solution has the advantages of easy availability of raw materials and relatively low prices, which is conducive to reducing the production cost of iron phosphate.

[0080] In some embodiments, the phosphate solution and hydrogen peroxide can be added for 20 to 60 minutes, such as 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes. The reaction time after the addition can be 1 hour to 2 hours, such as 1 hour, 1.5 hours or 2 hours. For example, the phosphate solution and hydrogen peroxide can be added for 50 minutes. The reaction time after the addition can be 1 hour.

[0081] In some embodiments, the conductivity of the rinse liquid after the primary amorphous ferric phosphate is rinsed can be, for example, 5 ms / cm, 4.5 ms / cm, 4 ms / cm, 3.5 ms / cm, 3 ms / cm, 2.5 ms / cm, 2 ms / cm, 1.5 ms / cm, 1 ms / cm or 0.5 ms / cm, etc. By controlling this condition, it is beneficial to reduce the impurity content of the amorphous ferric phosphate.

[0082] In some embodiments, the amorphous iron phosphate is slurried by adding water and phosphoric acid, and then the temperature is raised and aged to obtain an aged slurry, comprising:

[0083] Adding water and phosphoric acid to amorphous iron phosphate for slurry treatment to obtain an initial slurry;

[0084] The initial slurry is heated to 80°C to 100°C, and after the initial slurry changes color, the temperature is kept for 60min to 100min to obtain an aged slurry;

[0085] The P / Fe molar ratio of the added phosphoric acid to the amorphous iron phosphate is 0.2:1 to 0.3:1.

[0086] In some embodiments, amorphous ferric phosphate can be dispersed in water first, and then phosphoric acid is added. Dispersion can be carried out under stirring conditions, and the stirring speed can be exemplarily 400rpm to 600rpm, such as 400rpm, 450rpm, 500rpm, 550rpm or 600rpm. The dispersion time can be exemplarily 30min to 50min, such as 30min, 35min, 40min, 45min or 50min.

[0087] In some embodiments, the P / Fe molar ratio of phosphoric acid to amorphous iron phosphate can be set to 0.2:1, 0.25:1 or 0.3:1, etc., or any other value within the range of 0.2:1 to 0.3:1. Exemplarily, the P / Fe molar ratio of phosphoric acid to amorphous iron phosphate is 0.3:1.

[0088] By setting the P / Fe molar ratio of phosphoric acid to amorphous iron phosphate to 0.2:1 to 0.3:1, the problems of low product purity and low iron-phosphorus ratio caused by acid salt byproducts such as hydrogen ferric phosphate, dihydrogen ferric phosphate, and ammonium ferric sulfate produced under conditions of excessive phosphoric acid can be avoided. Among them, by setting the P / Fe molar ratio of phosphoric acid to amorphous iron phosphate to 0.3:1, a better effect can be obtained.

[0089] In some embodiments, the step of adding water and phosphoric acid to amorphous ferric phosphate for slurry treatment to obtain an initial slurry includes:

[0090] The amorphous ferric phosphate is slurried by adding water to obtain a slurry with a solid content of 15% to 30%;

[0091] Under stirring conditions, phosphoric acid is added into a slurry with a solid content of 15% to 30% to obtain an initial slurry.

[0092] The solid content of the slurry may be 15% to 30%, such as 15%, 18%, 20%, 22%, 25%, 28% or 30%, etc., or any other value within the range of 15% to 30%.

[0093] By adding phosphoric acid to the slurry with a solid content of 15% to 30%, it is beneficial to obtain a better dispersion effect in the first slurrying process, such as improving the dispersion degree and dispersion uniformity of large particle crystals and small particle crystals.

[0094] In some embodiments, the aging temperature can be controlled at 80°C to 100°C, that is, the initial slurry can be heated to 80°C, 85°C, 90°C, 95°C or 100°C, etc., or any other value within the range of 80 to 100°C. By controlling the aging temperature within the above range, the crystal transformation of amorphous iron phosphate can be achieved. Exemplarily, the aging temperature can be 90°C.

[0095] In some embodiments, the holding time after the initial slurry changes color can be 60min, 65min, 70min, 75min, 80min, 85min, 90min, 95min or 100min, etc., or any other value within the range of 60 to 100min. By keeping the temperature for another 60min to 100min after the initial slurry changes color, it can be ensured that the amorphous iron phosphate undergoes sufficient crystal transformation and improves the yield. Exemplarily, the initial slurry changes color and is kept warm for another 100min.

[0096] In some embodiments, the slurry washing of the aged slurry may be performed once or multiple times, for example, twice, three times, four times or more. Accordingly, a corresponding filter press may be performed after each slurry washing. Exemplarily, the solid content of the slurry washing may be 15% to 30%. Exemplarily, the slurry washing may be performed under stirring (the stirring speed may be 400rpm to 600rpm). Exemplarily, the slurry washing time may be 30min to 50min.

[0097] It can be understood that slurry washing of the aged slurry is beneficial to the dispersion of particles on the one hand and the removal of impurities on the other hand.

[0098] In some embodiments, after the aged slurry is subjected to slurry washing and filter pressing, the mother liquor obtained from the filter pressing can be recovered for recycling.

[0099] In some embodiments, in the process of obtaining the first slurry, the dosage relationship of the first filter cake and water satisfies that the solid content of the first slurry is 15% to 30%, such as 15%, 18%, 20%, 22%, 25%, 28% or 30%.

[0100] In some embodiments, the first filter cake may be dispersed in water before adding the first pH regulator. The first filter cake may be dispersed in water under stirring conditions, and the stirring speed may be illustratively 400 rpm to 600 rpm, such as 400 rpm, 450 rpm, 500 rpm, 550 rpm or 600 rpm. The dispersion time may be illustratively 30 min to 50 min, such as 30 min, 35 min, 40 min, 45 min or 50 min.

[0101] In some embodiments, the first pH adjuster is illustratively but not limitatively selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, sodium hydroxide and ammonia. The raw materials of the first pH adjuster are easily available and relatively cheap, which is conducive to reducing the production cost of iron phosphate.

[0102] In some embodiments, the pH value of the first slurry may be 3.0, 3.5, 4.0, 4.5 or 5.0, or any other value within the range of 3.0 to 5.0. By controlling the pH value of the first slurry to be between 3.0 and 5.0, it is possible to avoid the hydrolysis of ferric phosphate to produce ferric hydroxide byproducts due to excessively high pH values, and to help avoid excessively high iron-phosphorus ratios. Preferably, the pH value of the first slurry is between 3.5 and 4.5.

[0103] In some embodiments, the second filter cake may be rinsed only once, or multiple times, such as 2 times, 3 times, 4 times or more, as long as the conductivity of the rinse liquid after rinsing is less than or equal to 350 us / cm.

[0104] By controlling the conductivity of the second filter cake to be less than or equal to 350 us / cm, a rinsed and clean second filter cake can be obtained, which is beneficial for obtaining a finished iron phosphate product with higher purity and better consistency.

[0105] In some embodiments, the second filter cake after rinsing can be dried at a temperature of 100°C to 200°C (such as 100°C, 120°C, 150°C, 180°C or 200°C, etc.) for 0.5h to 1h (such as 0.5h, 0.8h or 1h, etc.), and specifically can be dried by flash evaporation. After drying, calcination can be performed at a temperature of 500°C to 700°C (such as 500°C, 550°C, 600°C, 650°C or 700°C, etc.) for 2h to 3h (such as 2h, 2.5h or 3h, etc.).

[0106] In a second aspect, the present invention provides a low-sulfur and high-iron-phosphorus iron phosphate, which is prepared by the above-mentioned preparation method of iron phosphate. The iron-phosphorus ratio of the low-sulfur and high-iron-phosphorus iron phosphate is 0.977-0.991, and / or the sulfur content is 18.55ppm-32.46ppm, and / or the specific surface area is 10.50m 2 / g~12.01m 2 / g.

[0107] In the technical scheme of the embodiment of the present application, amorphous iron phosphate is provided; water and phosphoric acid are added to the amorphous iron phosphate for slurry treatment, and then the temperature is raised for aging to obtain an aged slurry; the aged slurry is slurried and washed and filtered to obtain a first filter cake; water and a first pH regulator are added to the first filter cake for slurry washing to obtain a first slurry with a pH value range of 3.0 to 5.0, and then the first slurry is filtered to obtain a second filter cake; the second filter cake is rinsed, dried and calcined. The iron-phosphorus ratio prepared by the method is 0.977 to 0.991, the sulfur content is 18.55 ppm to 32.46 ppm, and the specific surface area is 10.50 m 2 / g~12.01m 2 / g.

[0108] Therefore, the iron phosphate prepared in the present application can overcome the technical problems existing in the prior art and has better electrochemical performance.

[0109] Furthermore, in some embodiments, the obtained iron phosphate has not only a higher iron-to-phosphorus ratio, a lower sulfur content, and a larger specific surface area, but is also pure-phase iron phosphate with a higher purity.

[0110] In a third aspect, an embodiment of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode active layer arranged on at least one side of the positive electrode collector, and the positive electrode active layer includes a lithium iron phosphate material prepared using the above-mentioned low-sulfur and high iron-phosphorus ratio iron phosphate as a precursor.

[0111] In this embodiment, the positive electrode plate includes a lithium iron phosphate material prepared by using the above-mentioned low-sulfur and high iron-phosphorus ratio iron phosphate as a precursor. The lithium iron phosphate material can inherit the characteristics of the above-mentioned iron phosphate such as low sulfur and high iron-phosphorus ratio, which is conducive to obtaining better electrochemical properties. Therefore, the positive electrode plate containing the lithium iron phosphate also has the advantage of excellent electrochemical properties.

[0112] In a fourth aspect, an embodiment of the present application provides a secondary battery comprising the above-mentioned positive electrode plate.

[0113] In this embodiment, the secondary battery includes the above-mentioned positive electrode plate, and thus has the advantage of excellent electrochemical performance.

[0114] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.

[0115] 1. Preparation method

[0116] Example 1

[0117] This embodiment provides a low-sulfur and high-iron-phosphorus iron phosphate, and the preparation method thereof includes:

[0118] Step (1): Dissolve ferrous sulfate, a byproduct of titanium dioxide, in water to obtain Fe 2+ A mixed slurry having a molar concentration of ions of 1.5 mol / L;

[0119] Step (2): adding ammonium bicarbonate to the mixed slurry to adjust the pH value of the mixed slurry to 5, and then filtering through a filter press, and standing the filtrate obtained by the filtration to clarify, thereby obtaining a ferrous sulfate solution;

[0120] Step (3): adding ammonium dihydrogen phosphate and hydrogen peroxide to the ferrous sulfate solution simultaneously, the adding time is 50 minutes, the molar ratio of phosphorus in the phosphate solution to iron in the ferrous sulfate solution is 1:1, the molar ratio of hydrogen peroxide in the hydrogen peroxide to iron in the ferrous sulfate solution is 1:1, and the reaction is continued for 1 hour after the addition is completed to obtain primary amorphous iron phosphate;

[0121] Step (4): filter-pressing and rinsing the primary amorphous iron phosphate until the conductivity of the rinsing liquid is 5 ms / cm, thereby obtaining amorphous iron phosphate;

[0122] Step (5): adding water to the rinsed amorphous iron phosphate at a solid content of 20%, slurrying and dispersing for 40 minutes at a stirring speed of 500 rpm (the first slurrying process), then adding phosphoric acid at a molar ratio of P:Fe=0.3:1, heating to 90°C, and keeping warm for 100 minutes after color change to obtain an aged slurry;

[0123] Step (6): filtering the aged slurry, adding water to the filter cake after filtering at a solid content of 20% for slurry washing, the slurry washing process is carried out at a stirring speed of 500 rpm for 40 minutes, and after washing, returning to the filter press for filtering to obtain a first filter cake and a mother liquor, wherein the mother liquor obtained by filtering can be collected for recycling;

[0124] Step (7): adding water to the first filter cake at a solid content ratio of 20%, performing slurry dispersion for 40 minutes at a stirring speed of 500 rpm (second slurry process), and then adding ammonium bicarbonate to obtain a first slurry with a pH value of 4; returning the first slurry to the filter press for filtration to obtain a second filter cake;

[0125] Step (8): rinsing the second filter cake multiple times until the conductivity of the rinsing liquid is 350 us / cm, thereby obtaining ferric phosphate dihydrate;

[0126] Step (9): Dry the rinsed dihydrate iron phosphate at 150° C. for 1 hour to obtain a dried product; calcine the dried product at 600° C. for 2 hours to obtain anhydrous iron phosphate.

[0127] Example 2

[0128] This embodiment provides a low-sulfur and high-iron-phosphorus iron phosphate, and the preparation method thereof includes:

[0129] Steps (1) to (4): the same as steps (1) to (4) of Example 1;

[0130] Step (5): adding water to the rinsed amorphous iron phosphate at a solid content of 15%, slurrying and dispersing for 30 minutes at a stirring speed of 400 rpm (the first slurrying process), then adding phosphoric acid at a molar ratio of P:Fe=0.3:1, heating to 90°C, and keeping the temperature for 100 minutes after the color changes to obtain an aged slurry;

[0131] Step (6): filtering the aged slurry, adding water to the filter cake after filtering at a solid content of 15% for slurry washing, the slurry washing process is carried out at a stirring speed of 400 rpm for 30 minutes, and after washing, returning to the filter press for filtering to obtain a first filter cake and a mother liquor, wherein the mother liquor obtained by filtering can be collected for recycling;

[0132] Step (7): adding a fixed amount of water to the first filter cake at a solid content ratio of 15%, slurrying and dispersing the mixture for 30 min at a stirring speed of 400 rpm (second slurrying process), and then adding ammonium bicarbonate to obtain a first slurry with a pH value of 5; returning the first slurry to the filter press for filtration to obtain a second filter cake;

[0133] Steps (8) and (9): Same as steps (8) and (9) of Example 1.

[0134] Example 3

[0135] This embodiment provides a low-sulfur and high-iron-phosphorus iron phosphate, and the preparation method thereof includes:

[0136] Steps (1) to (4): the same as steps (1) to (4) of Example 1;

[0137] Step (5): adding water to the rinsed amorphous iron phosphate at a solid content of 30%, slurrying and dispersing for 50 minutes at a stirring speed of 600 rpm (the first slurrying process), then adding phosphoric acid at a molar ratio of P:Fe=0.3:1, heating to 90°C, and keeping the temperature for 100 minutes after the color changes to obtain an aged slurry;

[0138] Step (6): filter pressing the aged slurry, adding water to the filter cake after the filter pressing at a solid content of 30% for slurry washing, the slurry washing process is carried out at a stirring speed of 600 rpm for 50 minutes, and after washing, returning to the filter press for filter pressing to obtain a first filter cake and a mother liquor, wherein the mother liquor obtained by the filter pressing can be collected for recycling;

[0139] Step (7): adding water to the first filter cake at a solid content ratio of 30%, slurrying and dispersing for 50 minutes at a stirring speed of 600 rpm (second slurrying process), and then adding ammonium bicarbonate to obtain a first slurry with a pH value of 3; returning the first slurry to the filter press for filtration to obtain a second filter cake;

[0140] Steps (8) and (9): Same as steps (8) and (9) of Example 1.

[0141] Example 4

[0142] The difference between this embodiment and embodiment 1 is that the ammonium bicarbonate in step (7) is replaced with sodium hydroxide.

[0143] Example 5

[0144] The difference between this embodiment and embodiment 1 is that the ammonium bicarbonate in step (7) is replaced with aqueous ammonia.

[0145] Example 6

[0146] The difference between this embodiment and embodiment 1 is that the ammonium bicarbonate in step (7) is replaced with ammonium carbonate.

[0147] Example 7

[0148] The difference between this embodiment and embodiment 1 is that the ammonium bicarbonate in step (7) is replaced with sodium bicarbonate.

[0149] Example 8

[0150] The difference between this embodiment and embodiment 1 is that the ammonium bicarbonate in step (7) is replaced with sodium carbonate.

[0151] Example 9

[0152] The difference between this embodiment and embodiment 1 is that in step (5), the P / Fe molar ratio of the added phosphoric acid to the amorphous iron phosphate is 0.2:1.

[0153] Example 10

[0154] The difference between this embodiment and embodiment 1 is that in step (3), the molar ratio of hydrogen peroxide in the hydrogen peroxide solution to the iron element in the ferrous sulfate solution is 0.5:1.

[0155] Embodiment 11

[0156] The difference between this embodiment and embodiment 1 is that in step (3), the molar ratio of hydrogen peroxide in the hydrogen peroxide solution to the iron element in the ferrous sulfate solution is 0.8:1.

[0157] Comparative Example 1

[0158] This comparative example provides a low-sulfur and high-iron-phosphorus iron phosphate, and the preparation method thereof comprises:

[0159] Steps (1) to (4): the same as steps (1) to (4) in Example 1;

[0160] Step (5): adding water to the rinsed amorphous ferric phosphate at a solid content of 20%, slurrying and dispersing for 40 minutes at a stirring speed of 500 rpm (the first slurrying process), adding phosphoric acid at a molar ratio of P:Fe=0.3:1, heating to 90°C, keeping the temperature for 100 minutes after the color changes, adding ammonium bicarbonate to adjust the pH to 4, and after aging, filtering and washing until the conductivity is 350 us / cm, to obtain ferric phosphate dihydrate;

[0161] Step (6): Same as step (9) in Example 1.

[0162] Comparative Example 2

[0163] The difference between this comparative example and Example 1 is that the pH value of the first slurry in step (7) in Example 1 is adjusted to 6.

[0164] Comparative Example 3

[0165] This comparative example provides a low-sulfur and high-iron-phosphorus iron phosphate, and the preparation method thereof comprises:

[0166] Steps (1) to (4): the same as steps (1) to (4) in Example 1;

[0167] Step (5): adding water to the rinsed amorphous ferric phosphate at a solid content of 20%, slurrying and dispersing for 40 minutes at a stirring speed of 500 rpm (the first slurrying process), then adding phosphoric acid at a molar ratio of P:Fe=0.3:1, heating to 90°C, and keeping the temperature for 100 minutes after the color changes. After aging, filtering and washing are performed until the conductivity is 350 us / cm, thereby obtaining ferric phosphate dihydrate;

[0168] Step (6): Same as step (9) in Example 1.

[0169] 2. Test methods and test results

[0170] 1. Property test of iron phosphate materials

[0171] The iron phosphate dihydrate obtained in step (8) of Example 1 and the iron phosphate dihydrate obtained in Comparative Example 1 were subjected to XRD tests respectively, and the results are as follows: Figure 1 shown.

[0172] Depend on Figure 1It can be seen that after the aging is completed in Example 1, the slurry is first filtered and washed, and after the filtration, ammonium bicarbonate is added to the slurry to adjust the pH value to 4, and then the filtration is continued to be rinsed until the conductivity is 350us / cm. At this time, the dihydrate iron phosphate obtained is pure phase FePO4·2H2O; compared with Comparative Example 1, ammonium bicarbonate is added at high temperature during the aging process to adjust the pH to 4. At this time, the temperature is very high, and crystal transformation is easy to occur in an alkaline environment. Therefore, the dihydrate iron phosphate obtained at this time is a pure phase (NH4)Fe2(PO4)2(OH)·2H2O, and the sintering process of dihydrate iron phosphate of this phase has an ammonia smell.

[0173] In addition, the anhydrous ferric phosphate obtained in step (9) of Example 1 and the anhydrous ferric phosphate obtained in step (6) of Comparative Example 3 were tested by scanning electron microscopy. The results (SEM images) are as follows: Figure 2 and Figure 3 shown.

[0174] Depend on Figure 2 and Figure 3 Comparison shows that the anhydrous iron phosphate obtained in Example 1 is more uniform in particles than the anhydrous iron phosphate obtained in Comparative Example 3, and there are holes between the particles, while the anhydrous iron phosphate obtained in Comparative Example 3 has obvious agglomeration and is denser. This corresponds to the specific surface area in Table 1 below. The specific surface area of ​​the anhydrous iron phosphate obtained in Example 1 is larger than that of the anhydrous iron phosphate obtained in Comparative Example 3. It can be seen that after aging, the slurry washing is performed by pressure filtration, and the slurry dispersion is continued after the pressure filtration, which is conducive to uniform dispersion of the particles. At the same time, the addition of alkali to adjust the pH to 4 reduces the formation of acid salts, reduces the surface energy, and effectively reduces the agglomeration between particles. Anhydrous iron phosphate with uniform particles, loose and porous particles, and a large specific surface area can be obtained, and the electrochemical performance of the lithium iron phosphate positive electrode material prepared by the anhydrous iron phosphate obtained in Example 1 is also improved.

[0175] Furthermore, in the present application, the anhydrous ferric phosphate obtained in Examples 1 to 16 and Comparative Examples 1 to 3 was tested for element content and specific surface area, and the results are shown in Table 1.

[0176] Among them, the sulfur content is detected by using an infrared carbon-sulfur meter, the specific surface area is detected by using a nitrogen adsorption method using a specific surface area tester to detect the specific surface area, the iron content is detected by using a potassium dichromate drop titration method, and the phosphorus content is detected by using a quinoline phosphomolybdic acid weight method to detect the phosphorus content.

[0177] Table 1 Performance indicators of anhydrous ferric phosphate in different embodiments and comparative examples

[0178]

[0179]

[0180] From Table 1 we can see that:

[0181] (1) The iron-phosphorus ratio of the iron phosphate prepared in Example 1 is in the range of 0.977 to 0.991, which is higher than that of Comparative Examples 1 and 3, indicating that the addition of alkali after aging, filter pressing and rinsing can effectively neutralize the acid and salt and improve the iron-phosphorus ratio;

[0182] (2) The iron-phosphorus ratio of the iron phosphate prepared in Example 2 is lower than that in Comparative Example 2. The iron-phosphorus ratio of the iron phosphate prepared in Comparative Example 2 is greater than 1, which indicates that the iron is not simply the iron in the iron phosphate, but also contains a small amount of other iron compounds, which may be iron hydroxide. This indicates that when the pH is adjusted to 6, the high pH easily causes the iron phosphate to hydrolyze and produce iron hydroxide byproducts;

[0183] (3) The specific surface area of ​​the iron phosphate obtained in the embodiment is 10.50 m 2 / g~12.01m 2 / g range, which is higher than that of Comparative Examples 1 and 3. On the one hand, the two slurryings disperse the large particles and the particle distribution is more uniform. On the other hand, the addition of alkali eliminates the acid salt and reduces the surface energy of the particles, making it difficult to agglomerate during the drying and calcining process.

[0184] (4) The specific surface area of ​​the iron phosphate obtained in Comparative Example 2 is very large, 13.61 m 2 / g, mainly because too high pH value can easily lead to hydrolysis of iron phosphate, producing iron hydroxide as a byproduct. Iron oxide is a very small colloidal particle.

[0185] (5) The sulfur content of the finished ferric phosphate products obtained in Example 1 and Comparative Example 2 is relatively low, indicating that the two slurrying processes can disperse large particles and reduce the particles. The addition of alkali can effectively eliminate acid salts and reduce the adsorption of sulfur.

[0186] 2. Property test of CR2032 button half-cell assembled with positive electrode

[0187] The anhydrous iron phosphate obtained in Examples 1 to 16 and Comparative Examples 1 to 3 was respectively prepared into positive electrode sheets according to the following methods, and then the obtained positive electrode sheets were assembled into CR2032 button half-cells, and the obtained CR2032 button half-cells were subjected to performance tests.

[0188] Preparation method: First, the iron phosphate and lithium source prepared in the above embodiments and comparative examples are sintered to obtain the corresponding lithium iron phosphate positive electrode material. Thereafter, the prepared lithium iron phosphate positive electrode material is mixed with conductive carbon powder and PVDF binder in a mass ratio of 90:5:5, and the slurry is coated on an aluminum foil, dried at 100°C and rolled with a double-roller machine. Then, a pole piece with a diameter of 14 mm is prepared with a punch, and the mass of the active substance is obtained by weighing and deducting the mass of the aluminum foil.

[0189] After drying the positive electrode, the CR2032 button half-cell was assembled in the UNlab inert gas first set box of Braun, Germany. The negative electrode shell, lithium sheet, electrolyte, diaphragm, electrolyte, positive electrode sheet, gasket, shrapnel, and positive electrode shell were assembled in this order. The Wuhan Blue Electric CT2001A battery test system was used to test the electrochemical performance of the CR2032 button half-cell, with a voltage range of 2.0-4.6V. The test results are shown in Table 2.

[0190] Table 2 Test results of CR2032 button half-cells of different embodiments and comparative examples

[0191]

[0192]

[0193] It can be seen from Table 2 that the CR2032 button half-cell corresponding to the iron phosphate provided in the embodiment of the present application can have a higher 0.1C charge specific capacity and 0.1C discharge specific capacity than the CR2032 button half-cell corresponding to the iron phosphate provided in the comparative example.

[0194] In summary, the present application is conducive to the preparation of iron phosphate with low sulfur content, high iron-phosphorus ratio, large specific surface area and high purity. The iron phosphate can be used to prepare lithium iron phosphate with good electrochemical performance, and the lithium iron phosphate can be further used to prepare positive electrode sheets and secondary batteries with good electrochemical performance.

[0195] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A method for preparing ferric phosphate with low sulfur and high iron-phosphorus ratio, characterized in that: include: Providing amorphous iron phosphate; The amorphous ferric phosphate is slurried by adding water to obtain a slurry with a solid content of 15% to 30%; Under stirring conditions, adding phosphoric acid to the slurry having a solid content of 15% to 30% to obtain an initial slurry; The initial slurry is heated to 80° C. to 100° C., and after the initial slurry changes color, the temperature is kept for 60 min to 100 min to obtain an aged slurry; wherein the P / Fe molar ratio of the added phosphoric acid to the amorphous iron phosphate is 0.2:1 to 0.3:1; The aged slurry is subjected to slurry washing and pressure filtering to obtain a first filter cake; Adding water and a first pH adjuster to the first filter cake for slurry washing to obtain a first slurry with a pH value ranging from 3.0 to 5.0, and then filtering the first slurry to obtain a second filter cake; The second filter cake is rinsed, dried, and calcined to prepare the low-sulfur and high-iron-phosphorus iron phosphate; The low-sulfur and high-iron-phosphorus ratio ferric phosphate obtained by the preparation method has an iron-phosphorus ratio of 0.977-0.991, a sulfur content of 18.55ppm-32.46ppm, and a specific surface area of ​​10.50m 2 / g~12.01m 2 / g.

2. The method for preparing ferric phosphate with low sulfur and high iron-phosphorus ratio according to claim 1, characterized in that: The preparation method of the amorphous ferric phosphate provided includes: Dissolving the titanium dioxide byproduct in water to obtain a mixed slurry; adding a second pH adjusting agent to the mixed slurry to adjust the pH value of the mixed slurry to 4.0-5.0, and then performing solid-liquid separation to obtain a ferrous sulfate solution; Mixing the ferrous sulfate solution, the phosphate solution and the hydrogen peroxide to obtain primary amorphous ferric phosphate; The primary amorphous iron phosphate is rinsed until the conductivity of the rinsing liquid is less than or equal to 5 ms / cm to obtain the amorphous iron phosphate.

3. The method for preparing ferric phosphate with low sulfur and high iron-phosphorus ratio according to claim 2, characterized in that: The molar ratio of phosphorus in the phosphate solution to iron in the ferrous sulfate solution is 1:1 to 1.1:1; And / or, the molar ratio of hydrogen peroxide in the hydrogen peroxide solution to iron in the ferrous sulfate solution is 0.5:1 to 1:

1.

4. The method for preparing ferric phosphate with low sulfur and high iron-phosphorus ratio according to claim 3, characterized in that: The solute in the phosphate solution is selected from at least one of diammonium phosphate and diammonium hydrogen phosphate; and / or, the first pH regulator is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, sodium hydroxide and ammonia water; And / or, the second pH adjuster is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate, sodium hydroxide and ammonia water.

5. The method for preparing ferric phosphate with low sulfur and high iron-phosphorus ratio according to any one of claims 1 to 4, characterized in that: The second filter cake is rinsed for multiple times until the conductivity of the rinsing liquid is less than or equal to 350 μs / cm, and then the second filter cake is dried and calcined to prepare the low-sulfur and high-iron-phosphorus ratio iron phosphate.

6. A low-sulfur and high iron-phosphorus ratio ferric phosphate, characterized in that: Prepared by the preparation method of ferric phosphate according to any one of claims 1 to 5; wherein, The iron-phosphorus ratio of the low-sulfur and high-iron-phosphorus iron phosphate is 0.977-0.991; and, the sulfur content of the low-sulfur and high-iron-phosphorus ratio iron phosphate is 18.55ppm to 32.46ppm; The specific surface area of ​​the low-sulfur and high-iron-phosphorus iron phosphate is 10.50 m 2 / g~12.01m 2 / g.

7. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector and a positive electrode active layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises a lithium iron phosphate material prepared by using the low-sulfur and high-iron-phosphorus ratio iron phosphate according to claim 6 as a precursor.

8. A secondary battery, characterized in that: The secondary battery comprises the positive electrode sheet according to claim 7.

Citation Information

Patent Citations

  • Method for producing ordinary zinc phosphate and caustic soda by using sodium hydrosulfite filtration residues

    CN102092697A

  • Method for preparing battery-grade iron phosphate by formed foil wastewater and iron phosphate prepared by method

    CN109399596A

  • Novel method capable of flexibly improving iron-phosphorus ratio of iron phosphate

    CN112142025A

  • Iron phosphate dihydrate with flexibly adjustable crystal structure and preparation method thereof

    CN113666350A

  • Battery-grade iron phosphate, preparation method therefor, and application thereof

    WO2022127323A1

Cited By

  • Iron phosphate having low sulfur content and high iron-phosphorus ratio, preparation method therefor, and use thereof