A kind of high strength concrete for building and preparation method thereof

By using a hydrophobic modified liquid and modified silica nanoparticles in concrete, combined with calcium gluconate, the corrosion problem of concrete during water penetration in the existing technology is solved, and the compressive strength and flexural strength are improved. , and enhanced corrosion resistance, suitable for extreme environments.

CN118184258BActive Publication Date: 2024-10-29JIANGSU UNIV OF SCI & TECH SUZHOU INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410284070.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-10-29
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Existing concrete still cannot effectively prevent corrosion damage caused by chloride ions and sulfate ions during water penetration, and the introduced corrosion inhibitors may reduce the compressive strength of concrete.

Method used

The hydrophobic modification liquid is mixed with modified silica, calcium gluconate and deionized water. By introducing nano-silica grafted with fluorine chains and cationic chains, the corrosion resistance and strength of the concrete are improved. The combination of calcium gluconate and Modified silica nanoparticles are compounded to enhance the strength and corrosion resistance of concrete.

Benefits of technology

It significantly improves the compressive strength and flexural strength of concrete, while enhancing its corrosion resistance, making it suitable for extreme environments such as inland saline soil and cold areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004738514480000071
    Figure BDA0004738514480000071
  • Figure BDA0004738514480000081
    Figure BDA0004738514480000081
Patent Text Reader

Abstract

The present invention relates to the field of concrete technology, and in particular to a high-strength concrete for construction and a preparation method thereof. The high-strength concrete for construction of the present invention is prepared from the following raw materials in parts by weight: 360-400 parts of cement, 1020-1150 parts of coarse aggregate, 690-760 parts of fine aggregate, 90-100 parts of fly ash, 10-12 parts of glass fiber, 10-12 parts of steel fiber, 6.2-6.8 parts of water reducer, 20-23 parts of hydrophobic modified liquid and 160-180 parts of water, wherein the hydrophobic modified liquid is obtained by mixing modified silica, calcium gluconate and deionized water. The high-strength concrete for construction of the present invention has excellent compressive strength, flexural strength and corrosion resistance, and can be applied to extreme environments such as inland saline soil and cold areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete, and in particular to a high-strength concrete for construction and a preparation method thereof. Background Art

[0002] Concrete is a porous material with nanometer to millimeter-scale micropores distributed on its surface. When water comes into contact with concrete, it will be adsorbed to the outer surface of the concrete by the capillary action of the micropores, and then gradually penetrate into the concrete structure. At this time, if the water contains chloride ions, sulfate ions and other ions that have a corrosive effect on concrete, they will also penetrate into the interior of the concrete with the water, causing corrosion damage to the concrete.

[0003] In the current research on improving the corrosion resistance of concrete, the preparation of cement with strong corrosion resistance is to increase the density of concrete and reduce the water penetration rate to improve the corrosion resistance, and the concrete surface coating protection is to prevent the direct contact between water and the concrete surface by coating to achieve the purpose of improving the corrosion resistance and durability of concrete. These methods reduce the penetration of water into concrete to a certain extent and improve the durability of concrete structure, but do not fundamentally change the hydrophilic nature of concrete.

[0004] Patent technology document CN116354651B discloses a corrosion-resistant and compression-resistant concrete and its preparation process, wherein the raw materials of the concrete include cement, fly ash, river sand, crushed stone, stone, high-efficiency water reducing agent, water and corrosion-resistant admixture, wherein the corrosion-resistant admixture includes multi-component corrosion-resistant agent, carboxylic acid-modified composite starch and amino-modified mesoporous silica, and the multi-component corrosion-resistant agent includes tannic acid, sodium gluconate and poly-L-aspartic acid. The addition of the corrosion-resistant agent in the invention is mainly to prevent or slow down the corrosion of steel bars in concrete, and chloride ions, sulfates, etc. will still penetrate into the concrete with water to cause corrosion damage to the concrete.

[0005] Patent document CN106277963B discloses a high-strength waterproof concrete. The invention adds sodium perfluorooctane sulfonate to the traditional concrete formula. However, the introduction of low surface energy perfluoro chains inhibits the hydration of cement in the concrete, reducing the cement hydration products compared to ordinary concrete without perfluoro chains, thereby causing a decrease in compressive strength. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a high-strength concrete for construction and a preparation method thereof, so as to provide a high-strength concrete with strong corrosion resistance.

[0007] Based on the above purpose, the present invention provides a high-strength concrete for construction, which is prepared from the following raw materials in parts by weight: 360-400 parts of cement, 1020-1150 parts of coarse aggregate, 690-760 parts of fine aggregate, 90-100 parts of fly ash, 10-12 parts of glass fiber, 10-12 parts of steel fiber, 6.2-6.8 parts of water reducer, 20-23 parts of hydrophobic modification liquid and 160-180 parts of water; the hydrophobic modification liquid is obtained by mixing modified silicon dioxide, calcium gluconate and deionized water; the modified silicon dioxide is obtained by co-grafting nano-silicon dioxide with tridecafluorooctyltrimethoxysilane and vinyltrimethoxysilane to obtain co-modified silicon dioxide, and then polymerizing methacryloyloxyethyltrimethylammonium chloride on the surface of the co-modified silicon dioxide through free radical copolymerization.

[0008] Preferably, the particle size of the coarse aggregate is 10-25 mm, and the particle size of the fine aggregate is 0.15-0.3 mm.

[0009] Preferably, the length of the glass fiber and the steel fiber is 20-30 mm.

[0010] Preferably, the cement is silicate cement, the coarse aggregate is crushed stone, and the fine aggregate is river sand.

[0011] Preferably, the water reducer is a polycarboxylic acid water reducer.

[0012] Preferably, the fly ash is Class II fly ash.

[0013] Preferably, the weight ratio of modified silicon dioxide, calcium gluconate and deionized water in the hydrophobic modification liquid is 5-10:1-3:20-40.

[0014] Preferably, the preparation steps of the modified silicon dioxide are:

[0015] S1: In a nitrogen atmosphere, nano-silica is dispersed in a mixed solution of anhydrous ethanol and deionized water, the pH is adjusted to 4-5, and then tridecafluorooctyltrimethoxysilane and vinyltrimethoxysilane are added, reacted at 70-75°C for 4-6h, washed with water, washed with alcohol, centrifuged, and dried to obtain co-modified silica;

[0016] S2: Under a nitrogen atmosphere, the co-modified silica is dispersed in anhydrous ethanol, and then methacryloyloxyethyl trimethyl ammonium chloride is added, the temperature is raised to 60-70°C, and ammonium persulfate is added dropwise. After the addition of ammonium persulfate is completed, the reaction is carried out for 6-8 hours, and the modified silica is obtained by washing with water, centrifuging, and drying.

[0017] Preferably, the weight ratio of the nano-silicon dioxide, anhydrous ethanol and deionized water, tridecafluorooctyltrimethoxysilane and vinyltrimethoxysilane in step S1 is 5-10:50-100:15-40:0.5-1:0.2-0.4;

[0018] Preferably, the weight ratio of the co-modified silica, ethanol, methacryloyloxyethyltrimethylammonium chloride and ammonium persulfate in step S2 is 5-10:20-50:2.5-8:0.05-0.1.

[0019] Preferably, the particle size of the nano-silicon dioxide is 200-500 nm.

[0020] Furthermore, the present invention also provides a method for preparing high-strength concrete for construction, comprising the following steps:

[0021] (1) mixing coarse aggregate, fine aggregate, fly ash, glass fiber and steel fiber to obtain a mixture;

[0022] (2) After cement, water and water reducing agent are mixed, the mixture and the hydrophobic modification liquid are added and stirred evenly to obtain high-strength concrete for construction.

[0023] Beneficial effects of the present invention:

[0024] (1) The present invention adds nano-silica grafted with fluorine chains and cationic chains into concrete, and by introducing fluorine bonds and cationic chains and utilizing the difference in chain lengths of cationic chains and fluorine chains, the corrosion resistance of concrete is improved, and its strength is also improved.

[0025] (2) The present invention cleverly uses calcium gluconate and modified silicon dioxide nanoparticles to jointly promote the strength and corrosion resistance of concrete.

[0026] (3) The high-strength concrete for construction of the present invention can be applied to extreme environments such as inland saline soil and cold regions. DETAILED DESCRIPTION

[0027] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0028] The sources and / or properties of the raw materials used in the examples and comparative examples of the present invention are as follows: nano-silicon dioxide was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. with the item number S433668; cement was PO42.5 ordinary Portland cement purchased from Guangdong Tapai Group Co., Ltd.

[0029] Example 1: A high-strength concrete for construction, the specific preparation steps are as follows:

[0030] (1) Under a nitrogen atmosphere, 11 g of nano-silica was dispersed in a mixed solution of 100 g of anhydrous ethanol and 30 g of deionized water, the pH was adjusted to 4.1, 1 g of tridecafluorooctyltrimethoxysilane and 0.4 g of vinyltrimethoxysilane were added, and the mixture was reacted at 70° C. for 4 h, washed three times with water, washed three times with alcohol, centrifuged, and dried to obtain co-modified silica;

[0031] (2) Under nitrogen atmosphere, 5 g of co-modified silica was dispersed in 20 g of anhydrous ethanol, and then 2.5 g of methacryloyloxyethyl trimethyl ammonium chloride was added, the temperature was raised to 60° C., and 0.05 g of ammonium persulfate was added dropwise. After the addition of ammonium persulfate was completed, the mixture was reacted for 6 h, washed with water, centrifuged, and dried to obtain modified silica;

[0032] (3) 5 g of modified silicon dioxide, 1 g of calcium gluconate and 20 g of deionized water were mixed and stirred to obtain a hydrophobic modified liquid;

[0033] (4) 1020 g of crushed stone, 690 g of river sand, 90 g of Class II fly ash, 10 g of glass fiber and 10 g of steel fiber were mixed to obtain a mixture;

[0034] (5) After mixing 360 g of cement, 160 g of water, and 6.2 g of polycarboxylate water reducer, add the mixture and 20 g of hydrophobic modification liquid, stir evenly, and obtain high-strength concrete for construction.

[0035] Example 2: A high-strength concrete for construction, the specific preparation steps are as follows:

[0036] (1) Under a nitrogen atmosphere, 15 g of nano-silica was dispersed in a mixed solution of 150 g of anhydrous ethanol and 55 g of deionized water, the pH was adjusted to 4.5, 1.5 g of tridecafluorooctyltrimethoxysilane and 0.6 g of vinyltrimethoxysilane were added, and the mixture was reacted at 73 ° C for 5 h, washed with water three times, washed with alcohol three times, centrifuged, and dried to obtain co-modified silica;

[0037] (2) Under nitrogen atmosphere, 7.5 g of co-modified silica was dispersed in 35 g of anhydrous ethanol, and then 5 g of methacryloyloxyethyl trimethyl ammonium chloride was added, the temperature was raised to 65° C., and 0.075 g of ammonium persulfate was added dropwise. After the addition of ammonium persulfate was completed, the mixture was reacted for 7 h, washed with water, centrifuged, and dried to obtain modified silica;

[0038] (3) 7.5 g of modified silicon dioxide, 2 g of calcium gluconate and 30 g of deionized water were mixed and stirred to obtain a hydrophobic modified liquid;

[0039] (4) 1035 g of crushed stone, 730 g of river sand, 95 g of Class II fly ash, 11 g of glass fiber and 11 g of steel fiber were mixed to obtain a mixture;

[0040] (5) After mixing 380 g of cement, 170 g of water, and 6.5 g of polycarboxylate water reducer, add the mixture and 22 g of hydrophobic modification liquid, stir evenly, and obtain high-strength concrete for construction.

[0041] Example 3: A high-strength concrete for construction, the specific preparation steps are as follows:

[0042] (1) Under a nitrogen atmosphere, 18 g of nano-silica was dispersed in a mixed solution of 170 g of anhydrous ethanol and 70 g of deionized water, the pH was adjusted to 4.7, 1.7 g of tridecafluorooctyltrimethoxysilane and 0.7 g of vinyltrimethoxysilane were added, and the mixture was reacted at 75° C. for 6 h, washed three times with water, washed three times with alcohol, centrifuged, and dried to obtain co-modified silica;

[0043] (2) Under a nitrogen atmosphere, 8 g of co-modified silica was dispersed in 40 g of anhydrous ethanol, and then 7 g of methacryloyloxyethyl trimethyl ammonium chloride was added, the temperature was raised to 70° C., and 0.08 g of ammonium persulfate was added dropwise. After the addition of ammonium persulfate was completed, the mixture was reacted for 8 h, washed with water, centrifuged, and dried to obtain modified silica;

[0044] (3) 8 g of modified silicon dioxide, 2 g of calcium gluconate and 30 g of deionized water were mixed and stirred to obtain a hydrophobic modified liquid;

[0045] (4) 1100 g of crushed stone, 750 g of river sand, 95 g of Class II fly ash, 12 g of glass fiber and 12 g of steel fiber were mixed to obtain a mixture;

[0046] (5) After mixing 390 g of cement, 180 g of water, and 6.8 g of polycarboxylate water reducer, add the mixture and 23 g of hydrophobic modification liquid, stir evenly, and obtain high-strength concrete for construction.

[0047] Example 4: A high-strength concrete for construction, the specific preparation steps are as follows:

[0048] (1) Under a nitrogen atmosphere, 20 g of nano-silica was dispersed in a mixed solution of 200 g of anhydrous ethanol and 80 g of deionized water, the pH was adjusted to 5, 2 g of tridecafluorooctyltrimethoxysilane and 0.8 g of vinyltrimethoxysilane were added, and the mixture was reacted at 75° C. for 6 h, washed three times with water, washed three times with alcohol, centrifuged, and dried to obtain co-modified silica;

[0049] (2) Under a nitrogen atmosphere, 10 g of co-modified silica was dispersed in 50 g of anhydrous ethanol, and then 8 g of methacryloyloxyethyl trimethyl ammonium chloride was added, the temperature was raised to 70° C., and 0.1 g of ammonium persulfate was added dropwise. After the addition of ammonium persulfate was completed, the mixture was reacted for 8 h, washed with water, centrifuged, and dried to obtain modified silica;

[0050] (3) 10 g of modified silicon dioxide, 3 g of calcium gluconate and 40 g of deionized water were mixed and stirred to obtain a hydrophobic modified liquid;

[0051] (4) 1150 g of crushed stone, 760 g of river sand, 100 g of Class II fly ash, 12 g of glass fiber and 12 g of steel fiber were mixed to obtain a mixture;

[0052] (5) After mixing 400 g of cement, 180 g of water, and 6.8 g of polycarboxylate water reducer, add the mixture and 23 g of hydrophobic modification liquid, stir evenly, and obtain high-strength concrete for construction.

[0053] Comparative Example 1: A concrete for construction, the specific preparation steps are as follows:

[0054] The difference between Comparative Example 1 and Example 2 is that tridecafluorooctyltrimethoxysilane in step (1) is replaced by vinyltrimethoxysilane.

[0055] Comparative Example 2: A concrete for construction, the specific preparation steps are as follows:

[0056] The difference between Comparative Example 2 and Example 2 is that the modified silica in step (3) is replaced by co-modified silica.

[0057] Comparative Example 3: A concrete for construction, the specific preparation steps are as follows:

[0058] The difference between Comparative Example 3 and Example 2 is that the calcium gluconate in step (3) is replaced by deionized water.

[0059] Performance Testing

[0060] Compressive strength: The concrete obtained in the embodiment and the comparative example was poured into a mold of 150 mm × 150 mm × 600 mm, and the square brick samples were obtained after curing for 28 days. The compressive properties of the square brick samples obtained in the embodiment and the comparative example were tested according to the compressive strength test in GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and the test results are shown in Table 1.

[0061] Flexural strength: The concrete obtained in the embodiment and the comparative example was poured into a mold of 150 mm × 150 mm × 150 mm, and the square brick samples were obtained after curing for 28 days. The flexural strength test of the square brick samples obtained in the embodiment and the comparative example was carried out according to the flexural strength test in GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", and the test results are shown in Table 1.

[0062] Freeze-thaw resistance: The concrete obtained in the embodiment and the comparative example was poured into a mold with an upper diameter of 175 mm, a lower diameter of 185 mm, and a height of 150 mm, and a square brick sample was obtained after curing for 28 days. According to GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", the square brick samples obtained in the embodiment and the comparative example were subjected to freeze-thaw resistance tests, and the test results are shown in Table 1.

[0063] Corrosion resistance test: The concrete obtained in the embodiment and the comparative example was wrapped with steel bars to prepare reinforced concrete specimens. The steel bars used in the specimens were No. 45 steel with a diameter of 8 mm, and the thickness of the concrete layer on the surface of the steel bars was 10 mm. The polarization curve of the specimens immersed in 3.5% NaCl solution for 30 days was detected using a PARSTAT2273 electrochemical workstation. The scanning frequency of the polarization curve measurement was 0.5 mV / s. The self-corrosion potential of the specimens was obtained according to the polarization curves. The test results are shown in Table 1.

[0064] Table 1 Performance test results

[0065]

[0066]

[0067] Data analysis shows that from Examples 1-4, it can be seen that the high-strength concrete for construction of the present invention has excellent mechanical properties and corrosion resistance, its compressive strength is not less than 53.5 MPa, and its flexural strength is not less than 5.9 MPa. At the same time, its freeze-thaw resistance is also relatively good, and it can be used in extreme environments such as inland saline soil and cold areas.

[0068] It can be seen from Example 2 and Comparative Examples 1-2 that the addition of nano-silica grafted with fluorine chains and cationic chains ensures that the concrete has good corrosion resistance while its compression and flexural properties can also be improved. This is mainly due to the effective avoidance of the problem of concrete strength reduction caused by the addition of fluorine chains. Due to the difference in chain lengths between cationic chains and fluorine chains, the cationic chains are located on the periphery, which helps to reduce the influence of fluorine chains on cement hydration products, thereby improving hydration performance and strength. At the same time, after the concrete is formed, the fluorine chains also help to improve its corrosion resistance.

[0069] It can be seen from Example 2 and Comparative Example 3 that calcium gluconate further improves the strength and corrosion resistance of concrete. On the one hand, calcium ions in calcium gluconate can penetrate into the cationic chains on the surface of modified silica to increase the intermolecular electrostatic repulsion, and calcium gluconate can also be interspersed between the cationic chains through ion exchange to increase the stretching degree of the cationic chains. During the hydration process, the contact area with the concrete raw materials can be increased, thereby improving the strength of the concrete. At the same time, the curling of the cationic chains is prevented, resulting in the inability of the fluorine chains in the concrete after molding to play a hydrophobic role. On the other hand, calcium gluconate has a lubricating effect, which can improve the dispersibility of modified silica in concrete. At the same time, calcium gluconate can also promote the hydration process and improve the strength of the concrete.

[0070] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0071] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A high-strength concrete for construction, characterized in that: Prepared from the following raw materials in parts by weight: 360-400 parts of cement, 1020-1150 parts of coarse aggregate, 690-760 parts of fine aggregate, 90-100 parts of fly ash, 10-12 parts of glass fiber, 10-12 parts of steel fiber, 6.2-6.8 parts of water reducing agent, 20-23 parts of hydrophobic modification liquid and 160-180 parts of water; The hydrophobic modified liquid is obtained by mixing modified silicon dioxide, calcium gluconate and deionized water; The weight ratio of modified silicon dioxide, calcium gluconate and deionized water in the hydrophobic modification liquid is 5-10:1-3:20-40; The modified silica is obtained by co-grafting tridecafluorooctyltrimethoxysilane and vinyltrimethoxysilane onto nano-silica to obtain co-modified silica, and then polymerizing methacryloyloxyethyltrimethylammonium chloride on the surface of the co-modified silica through free radical copolymerization; The preparation steps of the modified silicon dioxide are: S1: In a nitrogen atmosphere, nano-silica is dispersed in a mixed solution of anhydrous ethanol and deionized water, the pH is adjusted to 4-5, and then tridecafluorooctyltrimethoxysilane and vinyltrimethoxysilane are added, reacted at 70-75°C for 4-6h, washed with water, washed with alcohol, centrifuged, and dried to obtain co-modified silica; S2: Under a nitrogen atmosphere, the co-modified silica is dispersed in anhydrous ethanol, and then methacryloyloxyethyl trimethyl ammonium chloride is added, the temperature is raised to 60-70°C, and ammonium persulfate is added dropwise. After the addition of ammonium persulfate is completed, the reaction is carried out for 6-8 hours, and the modified silica is obtained by washing with water, centrifuging, and drying.

2. The high-strength concrete for construction according to claim 1, characterized in that: The cement is silicate cement, the coarse aggregate is crushed stone, and the fine aggregate is river sand.

3. The high-strength concrete for construction according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent.

4. The high-strength concrete for construction according to claim 1, characterized in that: The fly ash is Class II fly ash.

5. The high-strength concrete for construction according to claim 1, characterized in that: In the step S1, the weight ratio of nano-silicon dioxide, anhydrous ethanol and deionized water, tridecafluorooctyltrimethoxysilane and vinyltrimethoxysilane is 5-10:50-100:15-40:0.5-1:0.2-0.

4.

6. The high-strength concrete for construction according to claim 1, characterized in that: In the step S2, the weight ratio of the co-modified silica, ethanol, methacryloyloxyethyltrimethylammonium chloride and ammonium persulfate is 5-10:20-50:2.5-8:0.05-0.

1.

7. The high-strength concrete for construction according to claim 1, characterized in that: The particle size of the nano silicon dioxide is 200-500nm.

8. A method for preparing high-strength concrete for construction according to any one of claims 1 to 7, characterized in that: The steps include: (1) mixing coarse aggregate, fine aggregate, fly ash, glass fiber and steel fiber to obtain a mixture; (2) After cement, water and water reducing agent are mixed, the mixture and hydrophobic modified liquid are added and stirred evenly to obtain high-strength concrete for construction.

Citation Information

Patent Citations

  • A high-strength waterproof concrete

    CN106277963B

  • A corrosion-resistant and compressive-strength concrete and its preparation process

    CN116354651B

  • Steel fiber high-strength concrete and preparation method thereof

    CN111517718A

  • High-flow-state ultra-high performance concrete and preparation method thereof

    CN117623694A