A high-strength flame-retardant PC material and its production process
Through the coordinated cooperation of composite flame retardants and modified inorganic substrates in PC materials, the problem of insufficient anti-aging and flame retardant properties of existing PC materials is solved, significantly improving the flame retardant properties and anti-aging properties, and extending the The service life is guaranteed and the quality of the material is guaranteed.
Patent Information
- Application Number
- CN202410388617.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-04-01
AI Technical Summary
The existing high-strength wear-resistant PC materials have insufficient anti-aging and flame retardant properties, resulting in a shortened service life and an increased risk of fire hazards.
The inorganic substrate is used as the core, the modifier is used as the first shell layer, and the product generated by the chemical reaction between the reaction intermediate and 2,6-di-tert-butyl-4-methylphenol is the second shell layer, forming a composite flame retardant , and combined with glass fiber and toughener, porous nanomagnesium hydroxide with spherical flower-like structures was prepared by hydrothermal method. The modified inorganic substrate cooperated with chemical products to significantly improve flame retardant performance and anti-aging properties.
It significantly improves the flame retardant and anti-aging properties of PC materials, extends service life and ensures material quality, while maintaining good mechanical properties.
Smart Images

Figure CN118185273B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic engineering, in particular to a high-strength flame-retardant PC material and a production process thereof. Background Art
[0002] Polycarbonate, referred to as PC, is a widely used material with excellent comprehensive performance. It is common in life, such as beverage bottles, plastic bags, etc. It has high strength and elastic coefficient, high impact strength, wide operating temperature range, high transparency and free dyeing, low molding shrinkage, good dimensional stability, tasteless and odorless, harmless to the human body and in line with health and safety. Due to its many advantages, it is widely used in construction, automobiles, medicine, infrastructure, ships, aerospace and other fields.
[0003] The patent document with application number "CN202210948250.2" discloses a high-strength and wear-resistant PC material and its preparation process; it first uses microcrystalline cellulose as a raw material to prepare nanoscale nano-microcrystalline cellulose, and under the activation of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, replaces the hydroxyl groups on the surface of the nano-microcrystalline cellulose with epoxy groups, and reacts with high-pressure CO2 gas under catalytic conditions to achieve the ring-opening of the epoxy groups to obtain modified nanocellulose with carbonate monomers, and then uses a diol compound to generate polycarbonate, so that the modified nanocellulose can be effectively dispersed in the polycarbonate matrix and its binding ability is enhanced, so that the stress applied to the surface of the polycarbonate can be dispersed to avoid damage caused by stress concentration, thereby effectively enhancing the wear resistance and strength of the polycarbonate.
[0004] Although the PC material prepared in the above patent document has good wear resistance and mechanical strength, its anti-aging performance is relatively poor, which shortens its service life to a certain extent. Furthermore, its flame retardant performance is relatively insufficient. When a fire occurs accidentally during use, the losses and harms caused by the fire cannot be avoided. Therefore, the present invention provides a high-strength flame-retardant PC material and its production process to solve the above technical problems. Summary of the invention
[0005] The purpose of the present invention is to provide a high-strength flame-retardant PC material and a production process thereof. The produced PC material not only has good mechanical properties, but also has excellent anti-aging and flame-retardant properties, which effectively prolongs its service life while also ensuring its quality.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A high-strength flame-retardant PC material, composed of the following raw materials in parts by weight: 80-100 parts of PC resin, 35-45 parts of ABS resin, 20-30 parts of glass fiber, 1.0-1.8 parts of 3-aminopropyltriethoxysilane, 2-3 parts of potassium 3-phenylsulfonylbenzenesulfonate, 3-6 parts of nano titanium dioxide, 2-4 parts of pentaerythritol stearate, 3-5 parts of compatibilizer, 5-8 parts of toughening agent, 4-6 parts of composite flame retardant, 1.5-2.5 parts of antioxidant and 15-20 parts of inorganic filler;
[0008] The composite flame retardant has an inorganic substrate as a core, a modifier as a first shell, and a product generated by a chemical reaction between a reaction intermediate and 2,6-di-tert-butyl-4-methylphenol as a second shell, and has an obvious core-shell structure; the inorganic substrate is a porous nano magnesium hydroxide with a spherical flower-like structure;
[0009] Among them, PC resin uses bisphenol A polycarbonate with a molecular weight of 20,000 to 30,000;
[0010] ABS resin is a copolymer of acrylonitrile, butadiene and styrene, in which the percentage of butadiene is 20-30%;
[0011] The glass fiber is an alkali-free chopped glass fiber, and has a diameter of 5 to 10 μm and a chopped length of 3 to 5 mm.
[0012] Furthermore, the compatibilizer is selected from any one of PP-g-MA and PS-g-PMMA.
[0013] Furthermore, the antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
[0014] Furthermore, the inorganic filler is selected from any one of aluminum nitride, aluminum oxide, and silicon carbide; and its particle size is 5 to 15 μm.
[0015] Furthermore, the toughening agent is selected from any one of EMA, MBS, POE and high rubber powder.
[0016] Furthermore, the preparation method of the composite flame retardant is:
[0017] Step 1, tetraphosphoric acid and ethylene oxide are mixed and stirred in a mass ratio of 1:2-5, and reacted for 2-3 hours under the conditions of pressure lower than 0.15MPa and temperature of 50-60°C after inert gas replacement; after the reaction is completed, aminobenzene with a mass of 1-2 times that of ethylene oxide is added to the resulting component, and the reaction is kept at a pressure lower than 0.15MPa and a temperature of 60-80°C for 100-150 minutes; after the reaction is completed, the resulting product is a reaction intermediate;
[0018] Step 2: Add the modified inorganic substrate and 2,6-di-tert-butyl-4-methylphenol into ethanol in the dosage ratio of 0.002-0.004 g / mL and 0.003-0.005 g / mL respectively, mix and stir evenly, place the mixture in an oil bath, heat it to 60-70°C under magnetic stirring, and then add an ethanol dispersion of the reaction intermediate with a volume 3-5 times that of the mixed phase and a concentration of 0.005-0.008 g / mL to the mixed phase, and after uniform dispersion, keep warm for 30-40 hours under nitrogen protection; after the reaction is completed, evaporate the ethanol in the obtained product component, and then vacuum dry the obtained solid product at a temperature of 80-90°C to constant weight, and the obtained composite flame retardant is obtained.
[0019] Furthermore, the preparation method of the modified inorganic substrate comprises the following steps:
[0020] Ⅰ. Evenly disperse o-hydroxybenzoic acid in thionyl chloride at a solid-liquid ratio of 0.02-0.03 g / mL, reflux until no irritating gas escapes, and then stop the reaction; then evaporate the remaining thionyl chloride in the reaction system to obtain the modifier;
[0021] Ⅱ. Ultrasonic disperse the pretreated inorganic substrate in chloroform at a solid-liquid ratio of 0.01 to 0.02 g / mL, and add 40 to 60% of the mass of the pretreated inorganic substrate as the modifier and 3 to 5% of triethylamine in sequence; after mixing evenly, introduce nitrogen gas, and stir the reaction until no irritating gas escapes; then filter the resulting components, wash the filter cake alternately with chloroform and ethanol for 2 to 3 times, and then vacuum dry it to obtain the modified inorganic substrate.
[0022] Furthermore, the preparation method of the pretreated inorganic substrate is: the inorganic substrate is uniformly dispersed in N,N-dimethylformamide at a solid-liquid ratio of 0.005 to 0.01 g / mL, and then 3-aminopropyltrimethoxysilane with a mass of 20 to 30% of the inorganic substrate is added thereto, the mixture is mixed and stirred evenly, and then refluxed for 8 to 12 hours; after the reaction is completed, the obtained product components are separated into solid and liquid, and the obtained filter cake is washed with water and vacuum dried in turn to obtain the pretreated inorganic substrate.
[0023] Furthermore, the preparation method of the inorganic substrate is: add 20-35% of the mass of ethylene glycol to a 1-2 mol / L magnesium nitrate aqueous solution, mix and stir evenly, and then slowly add an equal volume of potassium hydroxide aqueous solution with a concentration of 2-4 mol / L to the obtained mixed solution, and then stir the reaction at a rate of 1000-2000 r / min for 20-30 hours. After the reaction is completed, the obtained precipitated product is aged for 3-6 hours and then filtered, the obtained filter cake is washed with deionized water until no nitrate ions are detected, and then washed with anhydrous ethanol for 2-3 times, and the solid powder obtained after washing is vacuum dried at a temperature of 70-100°C to constant weight, and the final result is the inorganic substrate.
[0024] A production process of a high-strength flame-retardant PC material comprises the following steps: accurately weighing various raw materials required for producing the high-strength flame-retardant PC material, and then drying them respectively at a temperature of 80 to 100° C. for 8 to 12 hours; after drying, mixing and stirring the various raw materials at a temperature of 50 to 65° C., transferring the obtained mixture into a twin-screw extruder for blending, and melt-extruding and granulating, and finally obtaining the high-strength flame-retardant PC material;
[0025] Among them, the temperatures of each zone of the twin-screw machine are: zone 1 225°C, zone 2 230°C, zone 3 245°C, zone 4 260°C, zone 5 270°C, zone 6 255°C, zone 7 265°C, zone 8 270°C, zone 9 275°C, head 280°C, and the speed is set to 320-450r / min.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] In the present invention, magnesium nitrate, ethylene glycol and potassium hydroxide are used as raw materials, and a porous nano magnesium hydroxide-inorganic substrate with a spherical flower-like structure is prepared by a hydrothermal method. Then, the inorganic substrate is pretreated with 3-aminopropyltrimethoxysilane, and the obtained pretreated inorganic substrate is ultrasonically dispersed in chloroform, and then chemically reacts with a modifier under the action of triethylamine, and finally the modifier is grafted on the surface of the pretreated inorganic substrate under the action of triethylamine. Due to the grafting of the modifier, the anti-ultraviolet aging performance of the inorganic substrate is significantly improved.
[0028] The obtained modified inorganic substrate and 2,6-di-tert-butyl-4-methylphenol are sequentially put into ethanol, mixed and stirred evenly, and then a reaction intermediate is added thereto, and the 2,6-di-tert-butyl-4-methylphenol retained in the pore structure of the inorganic substrate reacts chemically with the reaction intermediate through heat preservation reaction, and during the reaction process, the hydroxyl group in the 2,6-di-tert-butyl-4-methylphenol reacts chemically with the reaction intermediate to form a bond, and the nitrogen- and phosphorus-containing products obtained by the reaction of the two have good flame retardancy, and the densely staggered coating of the surface of the modified inorganic substrate forms a three-dimensional network envelope structure, and finally a composite flame retardant finished product is prepared. The obtained composite flame retardant has the inorganic substrate as the core, the modifier as the first shell layer, and the product generated by the chemical reaction of the reaction intermediate and 2,6-di-tert-butyl-4-methylphenol as the second shell layer, and has an obvious core-shell structure. Finally, the flame retardancy of the prepared PC material is significantly improved under the synergistic cooperation of the inorganic substrate and the generated chemical product. At the same time, the modifier and 2,6-di-tert-butyl-4-methylphenol work together to effectively improve the anti-aging properties of PC materials. The use of glass fiber and toughening agent also effectively guarantees the mechanical properties of PC materials.
[0029] In summary, the PC material produced by the present invention not only has good mechanical properties, but also has excellent anti-aging and flame retardant properties, which effectively prolongs its service life while also ensuring its quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the infrared spectrum of the reaction intermediate prepared in Example 1.
[0031] Figure 2 This is the infrared spectrum of the modifier prepared in Example 1. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A high-strength flame-retardant PC material, composed of the following raw materials in parts by weight: 80 parts of PC resin, 35 parts of ABS resin, 20 parts of glass fiber, 1.0 part of 3-aminopropyl triethoxysilane, 2 parts of potassium 3-phenylsulfonylbenzenesulfonate, 3 parts of nano titanium dioxide, 2 parts of pentaerythritol stearate, 3 parts of compatibilizer PP-g-MA, 5 parts of toughening agent EMA, 4 parts of composite flame retardant, 1.5 parts of antioxidant 1010 and 15 parts of aluminum nitride with a particle size of 5 μm;
[0035] The composite flame retardant has an inorganic substrate as a core, a modifier as a first shell, and a product generated by a chemical reaction between a reaction intermediate and 2,6-di-tert-butyl-4-methylphenol as a second shell, and has an obvious core-shell structure; the inorganic substrate is a porous nano magnesium hydroxide with a spherical flower-like structure;
[0036] Among them, PC resin uses bisphenol A polycarbonate with a molecular weight of 20,000;
[0037] ABS resin is a copolymer of acrylonitrile, butadiene, and styrene, in which the percentage of butadiene is 20%;
[0038] The glass fiber was an alkali-free chopped glass fiber, and had a diameter of 5 μm and a chopped length of 3 mm.
[0039] The preparation method of the composite flame retardant is:
[0040] Step 1, tetraphosphoric acid and ethylene oxide are mixed and stirred in a mass ratio of 1:2, and reacted for 2 hours under the conditions of pressure lower than 0.15MPa and temperature of 50°C after inert gas replacement; after the reaction is completed, aminobenzene in an amount equal to that of ethylene oxide is added to the resulting component, and the reaction is carried out at a pressure lower than 0.15MPa and a temperature of 60°C for 100 minutes; after the reaction is completed, the resulting product is a reaction intermediate;
[0041] Step 2: Add the modified inorganic substrate and 2,6-di-tert-butyl-4-methylphenol into ethanol in a dosage ratio of 0.002 g / mL and 0.003 g / mL respectively, mix and stir evenly, place the mixture in an oil bath, heat it to 60°C under magnetic stirring, and then add an ethanol dispersion of the reaction intermediate with a volume 3 times that of the mixture and a concentration of 0.005 g / mL to the mixed phase. After uniform dispersion, keep the mixture warm for 30 hours under nitrogen protection; after the reaction is completed, evaporate the ethanol in the resulting component, and then vacuum dry the resulting solid product at 80°C to constant weight, and the resulting composite flame retardant is obtained.
[0042] The preparation method of the modified inorganic substrate comprises the following steps:
[0043] Ⅰ. Disperse o-hydroxybenzoic acid evenly in thionyl chloride at a solid-liquid ratio of 0.02 g / mL, reflux until no irritating gas escapes, and then stop the reaction; then evaporate the remaining thionyl chloride in the reaction system to obtain the modifier;
[0044] Ⅱ. Ultrasonic disperse the pretreated inorganic substrate in chloroform at a solid-liquid ratio of 0.01 g / mL, and add 40% of the mass of the pretreated inorganic substrate and 3% of triethylamine in sequence; after mixing evenly, introduce nitrogen gas, and stir the reaction until no irritating gas escapes; then filter the resulting components, wash the filter cake alternately with chloroform and ethanol twice, and then vacuum dry it to obtain the modified inorganic substrate.
[0045] The preparation method of the pretreated inorganic substrate is as follows: the inorganic substrate is uniformly dispersed in N,N-dimethylformamide at a solid-liquid ratio of 0.005 g / mL, and then 3-aminopropyltrimethoxysilane with a mass of 20% of the inorganic substrate is added thereto, the mixture is stirred evenly and refluxed for 8 hours; after the reaction is completed, the obtained product components are separated into solid and liquid, and the obtained filter cake is washed with water and vacuum dried in turn to obtain the pretreated inorganic substrate.
[0046] The preparation method of the inorganic substrate is as follows: add 20% of the mass of ethylene glycol to a 1 mol / L magnesium nitrate aqueous solution, mix and stir evenly, then slowly drop an equal volume of 2 mol / L potassium hydroxide aqueous solution into the resulting mixture, and then stir and react at a rate of 1000 r / min for 20 hours. After the reaction is completed, the resulting precipitated product is aged for 3 hours and then filtered. The resulting filter cake is washed with deionized water until no nitrate ions are detected, and then washed twice with anhydrous ethanol. The solid powder obtained after washing is vacuum dried at 70°C to constant weight, and the final product is the inorganic substrate.
[0047] A production process of a high-strength flame-retardant PC material, comprising the following steps: accurately weighing various raw materials required for producing the high-strength flame-retardant PC material, and then drying them respectively at a temperature of 80° C. for 8 hours; after drying, mixing and stirring the various raw materials at a temperature of 50° C., transferring the obtained mixture into a twin-screw extruder for blending, and melt-extruding and granulating, and finally obtaining the high-strength flame-retardant PC material;
[0048] Among them, the temperatures of each zone of the twin-screw extruder are: zone 1 225℃, zone 2 230℃, zone 3 245℃, zone 4 260℃, zone 5 270℃, zone 6 255℃, zone 7 265℃, zone 8 270℃, zone 9 275℃, head 280℃, and the speed is set to 320r / min.
[0049] Example 2
[0050] The production process of the high-strength flame-retardant PC material in this embodiment is basically the same as that in Embodiment 1, except that: the specific ratio of the raw materials used in the high-strength flame-retardant PC material and the preparation method of the composite flame retardant are different; the specific ratio of the raw materials used in the high-strength flame-retardant PC material and the preparation method of the composite flame retardant in this embodiment are as follows:
[0051] A high-strength flame-retardant PC material is composed of the following raw materials in parts by weight: 90 parts of PC resin, 40 parts of ABS resin, 25 parts of glass fiber, 1.5 parts of 3-aminopropyltriethoxysilane, 2.5 parts of potassium 3-phenylsulfonylbenzenesulfonate, 5 parts of nano titanium dioxide, 3 parts of pentaerythritol stearate, 4 parts of compatibilizer PS-g-PMMA, 6 parts of toughening agent MBS, 5 parts of composite flame retardant, 2 parts of antioxidant 1076 and 16 parts of aluminum oxide with a particle size of 10 μm.
[0052] The preparation method of the composite flame retardant is:
[0053] Step 1: Mix tetraphosphoric acid and ethylene oxide in a mass ratio of 1:3 and stir evenly, and react for 2.5 hours at a pressure lower than 0.15 MPa and a temperature of 55°C after inert gas replacement; after the reaction is completed, add aminobenzene 1.5 times the mass of ethylene oxide to the resulting component, and keep the reaction at a pressure lower than 0.15 MPa and a temperature of 70°C for 120 minutes; after the reaction is completed, the resulting product is a reaction intermediate;
[0054] Step 2: Add the modified inorganic substrate and 2,6-di-tert-butyl-4-methylphenol into ethanol in a dosage ratio of 0.003 g / mL and 0.004 g / mL respectively, mix and stir evenly, place the mixture in an oil bath, heat it to 65°C under magnetic stirring, and then add an ethanol dispersion of the reaction intermediate with a volume 4 times that of the mixture and a concentration of 0.006 g / mL to the mixed phase. After uniform dispersion, keep the mixture warm for 35 hours under nitrogen protection; after the reaction is completed, evaporate the ethanol in the resulting component, and then vacuum dry the resulting solid product at 85°C to constant weight, and the resulting composite flame retardant is obtained.
[0055] The preparation method of the modified inorganic substrate comprises the following steps:
[0056] Ⅰ. Disperse o-hydroxybenzoic acid evenly in thionyl chloride at a solid-liquid ratio of 0.025 g / mL, reflux until no irritating gas escapes, and then stop the reaction; then evaporate the remaining thionyl chloride in the reaction system to obtain the modifier;
[0057] Ⅱ. Ultrasonic disperse the pretreated inorganic substrate in chloroform at a solid-liquid ratio of 0.015 g / mL, and add a modifier with a mass of 50% of the pretreated inorganic substrate and 4% of triethylamine in sequence; after mixing evenly, introduce nitrogen gas and stir the reaction until no irritating gas escapes; then filter the resulting components, wash the filter cake alternately with chloroform and ethanol twice, and then vacuum dry it to obtain the modified inorganic substrate.
[0058] The preparation method of the pretreated inorganic substrate is as follows: the inorganic substrate is uniformly dispersed in N,N-dimethylformamide at a solid-liquid ratio of 0.008 g / mL, and then 3-aminopropyltrimethoxysilane with a mass of 25% of the inorganic substrate is added thereto, the mixture is stirred evenly and refluxed for 10 hours; after the reaction is completed, the obtained product components are separated into solid and liquid, and the obtained filter cake is washed with water and vacuum dried in turn to obtain the pretreated inorganic substrate.
[0059] The preparation method of the inorganic substrate is as follows: add 30% of the mass of ethylene glycol to a 1.5 mol / L magnesium nitrate aqueous solution, mix and stir evenly, then slowly drop an equal volume of 3 mol / L potassium hydroxide aqueous solution into the resulting mixture, and then stir the mixture at a rate of 1500 r / min for 25 hours. After the reaction is completed, the precipitated product is aged for 5 hours and then filtered. The filter cake is washed with deionized water until no nitrate ions are detected, and then washed twice with anhydrous ethanol. The solid powder obtained after washing is vacuum dried at 80°C to constant weight, and the final product is the inorganic substrate.
[0060] Example 3
[0061] The production process of the high-strength flame-retardant PC material in this embodiment is basically the same as that in Embodiment 1, except that: the specific ratio of the raw materials used in the high-strength flame-retardant PC material and the preparation method of the composite flame retardant are different; the specific ratio of the raw materials used in the high-strength flame-retardant PC material and the preparation method of the composite flame retardant in this embodiment are as follows:
[0062] A high-strength flame-retardant PC material is composed of the following raw materials in parts by weight: 100 parts of PC resin, 45 parts of ABS resin, 30 parts of glass fiber, 1.8 parts of 3-aminopropyltriethoxysilane, 3 parts of potassium 3-phenylsulfonylbenzenesulfonate, 6 parts of nano titanium dioxide, 4 parts of pentaerythritol stearate, 5 parts of compatibilizer PP-g-MA, 8 parts of toughening agent POE, 6 parts of composite flame retardant, 2.5 parts of antioxidant 168 and 20 parts of silicon carbide with a particle size of 15 μm.
[0063] The preparation method of the composite flame retardant is:
[0064] Step 1, tetraphosphoric acid and ethylene oxide are mixed and stirred at a mass ratio of 1:5, and reacted for 3 hours at a pressure lower than 0.15 MPa and a temperature of 60°C after inert gas replacement; after the reaction is completed, aminobenzene with a mass twice that of ethylene oxide is added to the resulting component, and the mixture is kept warm for 150 minutes at a pressure lower than 0.15 MPa and a temperature of 80°C; after the reaction is completed, the resulting product is a reaction intermediate;
[0065] Step 2: Add the modified inorganic substrate and 2,6-di-tert-butyl-4-methylphenol into ethanol in a dosage ratio of 0.004 g / mL and 0.005 g / mL respectively, mix and stir evenly, place the mixture in an oil bath, heat to 70°C under magnetic stirring, and then add an ethanol dispersion of the reaction intermediate with a volume 5 times that of the mixture and a concentration of 0.008 g / mL to the mixed phase. After uniform dispersion, keep the mixture warm for 40 hours under nitrogen protection; after the reaction is completed, evaporate the ethanol in the resulting component, and then vacuum dry the resulting solid product at 90°C to constant weight, and the resulting composite flame retardant is obtained.
[0066] The preparation method of the modified inorganic substrate comprises the following steps:
[0067] Ⅰ. Disperse o-hydroxybenzoic acid uniformly in thionyl chloride at a solid-liquid ratio of 0.03 g / mL, reflux the reaction until no irritating gas escapes, and then stop the reaction; then evaporate the remaining thionyl chloride in the reaction system to obtain the modifier;
[0068] Ⅱ. Ultrasonic disperse the pretreated inorganic substrate in chloroform at a solid-liquid ratio of 0.02 g / mL, and add a modifier with a mass of 60% of the pretreated inorganic substrate and 5% of triethylamine in sequence; after mixing evenly, introduce nitrogen gas and stir the reaction until no irritating gas escapes; then filter the resulting components, wash the filter cake alternately with chloroform and ethanol for 3 times, and then vacuum dry it to obtain the modified inorganic substrate.
[0069] The preparation method of the pretreated inorganic substrate is as follows: the inorganic substrate is uniformly dispersed in N,N-dimethylformamide at a solid-liquid ratio of 0.01 g / mL, and then 3-aminopropyltrimethoxysilane with a mass of 30% of the inorganic substrate is added thereto, the mixture is stirred evenly and refluxed for 12 hours; after the reaction is completed, the obtained product components are separated into solid and liquid, and the obtained filter cake is washed with water and vacuum dried in turn to obtain the pretreated inorganic substrate.
[0070] The preparation method of the inorganic substrate is as follows: add 35% of the mass of ethylene glycol to a 2 mol / L magnesium nitrate aqueous solution, mix and stir evenly, then slowly drop an equal volume of 4 mol / L potassium hydroxide aqueous solution into the resulting mixture, and then stir the mixture at a rate of 2000 r / min for 30 hours. After the reaction is completed, the precipitated product is aged for 6 hours and then filtered. The filter cake is washed with deionized water until no nitrate ions are detected, and then washed three times with anhydrous ethanol. The solid powder obtained after washing is vacuum dried at 100°C to constant weight, and the final product is the inorganic substrate.
[0071] Comparative Example 1: The difference between this embodiment and embodiment 1 is that this embodiment uses an equal amount of modified inorganic substrate to replace the composite flame retardant.
[0072] Comparative Example 2: The difference between this embodiment and embodiment 1 is that in this embodiment, an equal amount of inorganic substrate is used to replace the composite flame retardant.
[0073] Comparative Example 3: The difference between this embodiment and embodiment 1 is that in this embodiment, an inorganic substrate is used instead of a modified inorganic substrate, that is, the preparation process of the modified inorganic substrate is omitted, and the inorganic substrate is directly used as a raw material for preparing the composite flame retardant.
[0074] Performance test: The relevant properties of the high-strength flame-retardant PC material samples provided in Examples 1 to 3 and Comparative Examples 1 to 3 were tested as follows:
[0075] 1. Mechanical properties test: The tensile properties test is carried out according to ISO527, the test equipment is the German Zwick Z010 electronic tensile machine, and the tensile speed is 50mm / min. The bending properties test is carried out according to ISO178, the test equipment is the Zwick Z010 electronic tensile machine, the span is 64mm, and the speed is 2mm / min.
[0076] 2. Flame retardant performance test: Limiting oxygen index (LOI) is the minimum oxygen concentration that maintains the combustion of the sample in a specific experimental environment, and is tested using the method specified in standard GB2406-93. Vertical burning test (UL-94) is tested using the method specified in standard GB / T2408-1996.
[0077] 3. Anti-aging performance: According to the plastic laboratory light source exposure test method GB / T16422.2-2014, place it in a xenon lamp exposure yellowing test box for irradiation, and then measure its yellowness index according to the HG / T3862-2006 plastic yellowness index test method to obtain its yellowing index △YI. The yellowing index △YI is an important indicator to characterize the light-oxidation aging performance. The smaller the △YI, the better the light yellowing resistance performance.
[0078] The test data obtained above are recorded in the following table:
[0079]
[0080]
[0081] By comparing and analyzing the relevant data in the table, it can be seen that the PC material produced by the present invention not only has good mechanical properties, but also has excellent anti-aging and flame retardant properties, which effectively prolongs its service life while also ensuring its quality. This shows that the high-strength flame-retardant PC material and its production process provided by the present invention have a broader market prospect and are more suitable for promotion.
[0082] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0083] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high-strength flame-retardant PC material, characterized in that: The invention is composed of the following raw materials in parts by weight: 80 to 100 parts of PC resin, 35 to 45 parts of ABS resin, 20 to 30 parts of glass fiber, 1.0 to 1.8 parts of 3-aminopropyl triethoxysilane, 2 to 3 parts of potassium 3-phenylsulfonylbenzenesulfonate, 3 to 6 parts of nano titanium dioxide, 2 to 4 parts of pentaerythritol stearate, 3 to 5 parts of compatibilizer, 5 to 8 parts of toughening agent, 4 to 6 parts of composite flame retardant, 1.5 to 2.5 parts of antioxidant and 15 to 20 parts of inorganic filler; The composite flame retardant has an inorganic substrate as a core, a modifier as a first shell, and a product generated by a chemical reaction between a reaction intermediate and 2,6-di-tert-butyl-4-methylphenol as a second shell, and has an obvious core-shell structure; the inorganic substrate is a porous nano magnesium hydroxide with a spherical flower-like structure; The inorganic filler is selected from any one of aluminum nitride, aluminum oxide, and silicon carbide; and its particle size is 5 to 15 μm; The preparation method of the composite flame retardant is: Step 1, tetraphosphoric acid and ethylene oxide are mixed and stirred in a mass ratio of 1:2-5, and reacted for 2-3 hours under the conditions of pressure lower than 0.15MPa and temperature of 50-60°C after inert gas replacement; after the reaction is completed, aminobenzene with a mass of 1-2 times that of ethylene oxide is added to the resulting component, and the reaction is kept at a pressure lower than 0.15MPa and a temperature of 60-80°C for 100-150 minutes; after the reaction is completed, the resulting product is a reaction intermediate; Step 2, respectively, adding the modified inorganic substrate and 2,6-di-tert-butyl-4-methylphenol into ethanol in a dosage ratio of 0.002-0.004 g / mL and 0.003-0.005 g / mL, mixing and stirring evenly, placing the resulting mixture in an oil bath, heating to 60-70° C. under magnetic stirring, and then adding an ethanol dispersion of a reaction intermediate with a volume 3-5 times that of the resulting mixture and a concentration of 0.005-0.008 g / mL to the resulting mixed phase, and then evenly dispersing the resulting mixture under nitrogen protection for 30-40 hours of heat preservation reaction; after the reaction is completed, ethanol in the resulting product components is evaporated, and then the resulting solid product is vacuum dried at a temperature of 80-90° C. to a constant weight, and the resulting composite flame retardant is obtained; The preparation method of the modified inorganic substrate comprises the following steps: Ⅰ. Evenly disperse o-hydroxybenzoic acid in thionyl chloride at a solid-liquid ratio of 0.02-0.03 g / mL, reflux until no irritating gas escapes, and then stop the reaction; then evaporate the remaining thionyl chloride in the reaction system to obtain the modifier; Ⅱ. Ultrasonic dispersion of the pretreated inorganic substrate in chloroform at a solid-liquid ratio of 0.01 to 0.02 g / mL, and sequential addition of a modifier of 40 to 60% by mass of the pretreated inorganic substrate and 3 to 5% of triethylamine; nitrogen is introduced after uniform mixing, and the reaction is stirred until no irritating gas escapes; the resulting components are then filtered, and the resulting filter cake is washed alternately with chloroform and ethanol for 2 to 3 times, and then vacuum dried to obtain the modified inorganic substrate; The preparation method of the pretreated inorganic substrate is as follows: the inorganic substrate is uniformly dispersed in N,N-dimethylformamide at a solid-liquid ratio of 0.005 to 0.01 g / mL, and then 3-aminopropyltrimethoxysilane is added thereto with a mass of 20 to 30% of the inorganic substrate, and the mixture is stirred evenly and then refluxed for reaction for 8 to 12 hours; after the reaction is completed, the obtained product components are separated into solid and liquid, and the obtained filter cake is washed with water and vacuum dried in turn to obtain the pretreated inorganic substrate.
2. The high-strength flame-retardant PC material according to claim 1, characterized in that: The compatibilizer is selected from any one of PP-g-MA and PS-g-PMMA.
3. The high-strength flame-retardant PC material according to claim 1, characterized in that: The antioxidant is selected from any one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
4. The high-strength flame-retardant PC material according to claim 1, characterized in that: The toughening agent is selected from any one of EMA, MBS, POE and high-rubber powder.
5. The high-strength flame-retardant PC material according to claim 1, characterized in that: The preparation method of the inorganic substrate is as follows: add ethylene glycol of 20 to 35% by mass to a 1 to 2 mol / L magnesium nitrate aqueous solution, mix and stir evenly, slowly drop an equal volume of potassium hydroxide aqueous solution with a concentration of 2 to 4 mol / L into the obtained mixed solution, then stir and react at a rate of 1000 to 2000 r / min for 20 to 30 hours, and after the reaction is completed, age the obtained precipitated product for 3 to 6 hours and then filter it, wash the obtained filter cake with deionized water until no nitrate ions are detected, then wash it with anhydrous ethanol for 2 to 3 times, and vacuum dry the solid powder obtained after washing at a temperature of 70 to 100° C. to constant weight, and finally obtain the inorganic substrate.
6. A production process for a high-strength flame-retardant PC material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: accurately weighing the raw materials required for producing the high-strength flame-retardant PC material, and then drying them at a temperature of 80 to 100° C. for 8 to 12 hours respectively; after drying, mixing and stirring the raw materials at a temperature of 50 to 65° C., transferring the obtained mixture into a twin-screw extruder for blending, and melt-extruding and granulating, and finally obtaining the high-strength flame-retardant PC material; Among them, the temperatures of each zone of the twin-screw extruder are: 225°C for zone 1, 230°C for zone 2, 245°C for zone 3, 260°C for zone 4, 270°C for zone 5, 255°C for zone 6, 265°C for zone 7, 270°C for zone 8, 275°C for zone 9, 280°C for the die head, and the speed is set to 320-450r / min.
Citation Information
Patent Citations
High-strength wear-resistant PC material and preparation process thereof
CN115109403A
Halogen-free flame retardant ABS resin and preparation method thereof
CN103160058A
Antibacterial plastic film and production process thereof
CN115304863A
Oligomeric phosphate polyol and preparation method thereof
CN115557988A
Alkyl phosphate oligomer preparation system and preparation method thereof
CN115672230A