Light diffusion polypropylene polycarbonate composite material and preparation method thereof

By mixing homopolypropylene and polycarbonate in a specific proportion in the composite material and adding components such as talc powder, the problem of difficult to take into account both optical and mechanical properties in the prior art is solved, and efficient light diffusion and mechanical properties are achieved Performance improvement simplifies the production process.

CN118931043APending Publication Date: 2024-11-12NINGBO GONEO PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226976.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing composite materials are difficult to take into account good optical and mechanical properties, resulting in fragility, shrinkage, deformation, and aging of products such as lamps and other products, as well as low production efficiency and high cost.

Method used

Using light-diffusion polypropylene polycarbonate composite material, by mixing homopolymer polypropylene and polycarbonate in a specific proportion, forming a heterogeneous system, adding talc powder, compatible agents, ultraviolet light absorbers and antioxidants, improve the The refractive and scattering effects, mechanical properties and resistance to UV aging of composite materials.

Benefits of technology

The good optical and mechanical properties of the composite material are achieved, and the transparency, thermal aging resistance and service life are improved, while simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025485480000111
    Figure BDA0005025485480000111
  • Figure BDA0005025485480000112
    Figure BDA0005025485480000112
  • Figure BDA0005025485480000121
    Figure BDA0005025485480000121
Patent Text Reader

Abstract

The invention relates to the technical field of composite materials, in particular to a light diffusion polypropylene polycarbonate composite material and a preparation method thereof. The light diffusion polypropylene polycarbonate composite material is prepared from the following raw materials in parts by weight: 90 to 110 parts of homo-polypropylene, 1 to 5 parts of polycarbonate, 3 to 6 parts of compatilizer, 0.5 to 1 part of talcum powder, 0.2 to 0.4 part of ultraviolet absorbent and 0.1 to 0.3 part of antioxidant, the preparation method comprises the steps of raw material mixing and granulation. The photodiffusion polypropylene polycarbonate composite material has good optical performance and mechanical performance, and the preparation method is simple and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, in particular to a light diffusion polypropylene polycarbonate composite material and a preparation method thereof. Background Art

[0002] When various lamps are used, they usually need to use decorative panels to transmit light, so as to improve the glare caused by the over-concentration of light from the light source. The decorative panels provided by the related art also need to be provided with a high-fog light diffuser in the inner layer to fully disperse the light and improve the glare problem; however, this method requires the separate production of two parts, the decorative panel and the light diffuser, which has low production efficiency and increases costs. Therefore, in order to improve the above problems, there is a related art that improves composite materials and uses composite materials to prepare decorative panels with light diffusion effects, so as to integrate the light diffuser and the decorative panel into a whole.

[0003] However, the composite materials provided by the related technology are difficult to achieve both good optical and mechanical properties. Summary of the invention

[0004] The object of the present invention is to provide a light-diffusing polypropylene-polycarbonate composite material and a preparation method thereof. The light-diffusing polypropylene-polycarbonate composite material can take into account both good optical properties and mechanical properties, and the preparation method is simple and easy to operate.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a light diffusion polypropylene polycarbonate composite material. The raw materials of the light diffusion polypropylene polycarbonate composite material include, by weight:

[0007] Homopolymer polypropylene 90-110 parts;

[0008] 1-5 parts of polycarbonate;

[0009] 3 to 6 parts of compatibilizer;

[0010] 0.5-1 part of talcum powder;

[0011] 0.2-0.4 parts of ultraviolet light absorber;

[0012] Antioxidant 0.1-0.3 parts.

[0013] In an optional embodiment, the weight ratio of polycarbonate to homopolypropylene is 1% to 5%.

[0014] In an optional embodiment, the particle size of the polycarbonate in the light diffusing polypropylene-polycarbonate composite material is 0.40-5.0 μm.

[0015] In an alternative embodiment, the homopolypropylene has a refractive index less than the refractive index of the polycarbonate.

[0016] In an optional embodiment, the refractive index of homopolypropylene is 1.40-1.50; the refractive index of polycarbonate is 1.55-1.60.

[0017] In an optional embodiment, the light transmittance of the homopolypropylene is 80-85%, the haze of the homopolypropylene is 10-16%, and the melt flow rate of the homopolypropylene is 1-3 g / 10 min (conditions: 230° C., 2.16 kg);

[0018] The light transmittance of the polycarbonate is 86 to 90%, the haze of the polycarbonate is 1 to 5%, and the melt flow rate of the polycarbonate is 10 to 15 g / 10 min (conditions: 300° C., 1.2 kg).

[0019] In an optional embodiment, the mesh size of the talc powder is 4500-5500 mesh, and the refractive index of the talc powder is 1.51-1.53.

[0020] In an optional embodiment, the ultraviolet light absorber includes at least one of 2-hydroxy-4-n-octyloxybenzophenone, tris(1,2,2,6,6-pentamethylpiperidinol)phosphite, and benzotriazole ultraviolet light absorbers; and / or,

[0021] The compatibilizer includes polypropylene grafted with maleic anhydride, wherein the grafting rate of maleic anhydride is 1-2%.

[0022] In an optional embodiment, the ultraviolet light absorber includes 2-hydroxy-4-n-octyloxybenzophenone, tris(1,2,2,6,6-pentamethylpiperidinol)phosphite and a benzotriazole ultraviolet light absorber in a mass ratio of (0.8-1.2):(0.8-1.2):(0.8-1.2).

[0023] In a second aspect, the present invention further provides a method for preparing a light-diffusing polypropylene-polycarbonate composite material, comprising: mixing raw materials of the light-diffusing polypropylene-polycarbonate composite material and granulating the raw materials.

[0024] The present invention has the following beneficial effects:

[0025] A small amount of polycarbonate PC is added to the light-diffusing polypropylene-polycarbonate composite material provided by the embodiment of the present invention and mixed with homopolymer polypropylene PP to form a heterogeneous system. PC exists in PP as a light scattering agent to form an island structure, thereby improving the refraction and scattering effects of the composite material; moreover, the addition of polycarbonate PC can also provide good mechanical properties, heat resistance and dimensional stability, that is, it can improve the mechanical properties of the composite material.

[0026] The addition of talcum powder can play a good role in nucleation and diffusion, so as to improve the transparency of the composite material and the overall diffusion effect of the composite material, and improve the problem of uneven light transmittance and unstable mechanical properties caused by agglomeration in the composite material.

[0027] The addition of compatibilizer can improve the compatibility of homopolymer polypropylene and polycarbonate, and at the same time can improve the overall polarity of the composite material, which is helpful for bonding.

[0028] The addition of UV absorbers can improve the composite material's ability to resist UV aging, delay the degradation of the composite material, and increase its lifespan. The addition of antioxidants can improve the composite material's resistance to thermal aging degradation.

[0029] The light-diffusing polypropylene-polycarbonate composite material prepared by the preparation method provided in the embodiment of the present invention includes all the aforementioned beneficial effects, and the preparation method is simple and easy to operate. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0031] The light diffusion material provided by the related technology usually uses a transparent resin as a base material, and adds light scattering agent particles to the base material to achieve light scattering through the refractive index difference between the two; however, this light diffusion material cannot take into account both light diffusion performance and mechanical properties, and the resulting lampshades and other products are prone to problems such as easy breakage, easy shrinkage and deformation, easy aging, and short life.

[0032] In order to improve the above problems, the present disclosure provides a light diffusion polypropylene polycarbonate composite material. The raw materials of the light diffusion polypropylene polycarbonate composite material include, by weight: 90 to 110 parts of homopolymer polypropylene, for example: 90 parts, 95 parts, 100 parts, 105 parts, 110 parts, etc., which are not specifically limited here; 1 to 5 parts of polycarbonate, for example: 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc., which are not specifically limited here; 3 to 6 parts of compatibilizer, for example: 3 parts, 4 parts, 5 parts, 6 parts, etc., are not specifically limited here; talc 0.5-1 parts, for example: 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, etc., are not specifically limited here; ultraviolet light absorber 0.2-0.4 parts, for example: 0.2 parts, 0.3 parts, 0.4 parts, etc., are not specifically limited here; antioxidant 0.1-0.3 parts, for example: 0.1 parts, 0.2 parts, 0.3 parts, etc., are not specifically limited here.

[0033] A small amount of polycarbonate PC is added to the light-diffusing polypropylene polycarbonate composite material and mixed with homopolymer polypropylene PP to form a heterogeneous system. PC exists in PP as a light scattering agent to form an island structure, thereby improving the refraction and scattering effects of the composite material; moreover, the addition of polycarbonate PC can also provide good mechanical properties, heat resistance and dimensional stability, that is, it can improve the mechanical properties of the composite material.

[0034] The addition of talcum powder can play a good role in nucleation and diffusion, so as to improve the transparency of the composite material and the overall diffusion effect of the composite material, and improve the problem of uneven light transmittance and unstable mechanical properties caused by agglomeration in the composite material.

[0035] The addition of compatibilizer can improve the compatibility of homopolymer polypropylene and polycarbonate, and at the same time can improve the overall polarity of the composite material, which is helpful for bonding.

[0036] The addition of UV absorbers can improve the composite material's ability to resist UV aging, delay the degradation of the composite material, and increase its lifespan. The addition of antioxidants can improve the composite material's resistance to thermal aging degradation.

[0037] The homopolymer polypropylene brand can be selected as needed, for example: R520Y, etc., which is not specifically limited here. Homopolymer polypropylene PP has good transparency, mechanical properties and processability, and has a low density, and can be used to prepare various light diffusion devices, such as: lampshades, etc.

[0038] The polycarbonate brand can be selected as needed, for example: weather-resistant PC IV1900R, etc., which is not specifically limited here. Polycarbonate PC has good mechanical properties, heat resistance and dimensional stability, and is a transparent thermoplastic with excellent comprehensive properties; mixing polycarbonate and homopolymer polypropylene can also make the composite material have a low melt index and high viscosity, and can be processed by injection blowing process.

[0039] Optionally, the weight ratio of polycarbonate to homopolypropylene is 1% to 5%, for example: 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 4.9%, 5%, etc., which are not specifically limited here. Due to the large difference in molecular chain structure and polarity between PP and PC, stratification and incompatibility will occur when the two are blended in large mass fractions. Therefore, optimizing the amount of PC added can effectively improve the incompatibility problem between the two, and make full use of PC as a light scattering agent in PP to improve the refraction and scattering effects of the composite material.

[0040] Optionally, the particle size of polycarbonate in the light-diffusing polypropylene polycarbonate composite material is 0.40 to 5.0 μm, for example: 0.40 μm, 0.41 μm, 0.45 μm, 0.50 μm, 0.70 μm, 1.0 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.0 μm, 2.4 μm, 2.7 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.2 μm, 4.5 μm, 4.9 μm, 5.0 μm, etc., which is not specifically limited here. A small amount of polycarbonate is mixed into a large amount of homopolymer polypropylene. The lower the content of polycarbonate, the smaller the particle size of the polycarbonate in the composite material. For example, when the mass percentage of polycarbonate is about 1%, the particle size of the polycarbonate in the mixture is approximately 0.41 microns. When the mass percentage of polycarbonate is about 5%, the particle size of the polycarbonate in the mixture is approximately 4.9 microns.

[0041] Optionally, in order to make the light-diffusing polypropylene-polycarbonate composite material have good optical properties; the refractive index of homopolymer polypropylene is smaller than that of polycarbonate, so that light scattering can be stably achieved through two materials with different refractive indices, that is, the difference in refractive index of PC and PP to light can be utilized to achieve the effect of light diffusion.

[0042] Furthermore, the refractive index of homopolypropylene is 1.40 to 1.50, for example, 1.40, 1.42, 1.45, 1.48, 1.50, etc., which is not specifically limited here; the refractive index of polycarbonate is 1.55 to 1.60, for example, 1.55, 1.56, 1.57, 1.58, 1.59, 1.60, etc., which is not specifically limited here.

[0043] Homopolymer polypropylene is a material with high light transmittance, low haze, and low melt flow rate; optionally, the light transmittance of homopolymer polypropylene is 80-85% (for example: 80%, 81%, 82%, 83%, 84%, 85%, etc., not specifically limited here), the haze of homopolymer polypropylene is 10-16% (for example: 10%, 11%, 12%, 13%, 14%, 15%, 16%, etc., not specifically limited here), and the melt flow rate of homopolymer polypropylene is 1-3g / 10min (condition: 230°C, 2.16kg), for example: 1g / 10min, 2g / 10min, 3g / 10min, etc., not specifically limited here. In this way, the light transmittance and light diffusion of the light diffusion polypropylene polycarbonate composite material can be ensured, while ensuring that the light diffusion polypropylene polycarbonate composite material has a low melt index, so that it can be processed by a blow molding process.

[0044] Optionally, the light transmittance of polycarbonate is 86-90% (for example: 86%, 87%, 88%, 89%, 90%, etc., not specifically limited herein), the haze of polycarbonate is 1-5% (for example: 1%, 2%, 3%, 4%, 5%, etc., not specifically limited herein), and the melt flow rate of polycarbonate is 10-15 g / 10 min (conditions: 300°C, 1.2 kg), for example: 10 g / 10 min, 11 g / 10 min, 12 g / 10 min, 13 g / 10 min, 14 g / 10 min, 15 g / 10 min, etc., not specifically limited herein. Mixing a small amount of polycarbonate with a relatively high melt flow rate into homopolymer polypropylene with a low melt flow rate will not only not adversely affect the blow molding performance of the light-diffusing polypropylene-polycarbonate composite material, but also ensure the dimensional stability of the light-diffusing polypropylene-polycarbonate composite material, that is, improve the problem that the light-diffusing polypropylene-polycarbonate composite material is prone to shrinkage and deformation after molding, for example: improve the problem that the lampshade prepared from the light-diffusing polypropylene-polycarbonate composite material cannot be assembled on the lamp body due to shrinkage and deformation. The high light transmittance and low haze of polycarbonate can ensure the good light transmittance and light diffusion of the light-diffusing polypropylene-polycarbonate composite material.

[0045] Optionally, the compatibilizer includes PP-g-MAH polypropylene grafted with maleic anhydride, wherein the maleic anhydride grafting rate is 1-2%, for example: 1%, 1.2%, 1.5%, 1.7%, 2%, etc., which is not specifically limited here.

[0046] Optionally, the particle size of talcum powder is about 3 microns, and the whiteness is greater than or equal to 95%; wherein, the mesh number of talcum powder is 4500-5500 mesh, for example: 4500 mesh, 4800 mesh, 5000 mesh, 5300 mesh, 5500 mesh, etc., which are not specifically limited here. A small amount of talcum powder can induce the nucleation of PP and improve transparency; if the mesh number of talcum powder is too small (large particle size), large particle impurities are likely to appear, resulting in uneven mixing of the composite material and inability to evenly diffuse light; if the mesh number of talcum powder is too large (small particle size), it is too fine, easy to agglomerate, uneven dispersion, and inability to evenly diffuse light.

[0047] Furthermore, talc powder crystals are in pseudo-hexagonal or rhombic flakes, with a refractive index of 1.51 to 1.53, for example, 1.51, 1.52, 1.53, etc., which are not specifically limited here; talc powder can also refract light to improve the overall diffusion effect in the composite material.

[0048] Optionally, the ultraviolet light absorber includes at least one of 2-hydroxy-4-n-octyloxybenzophenone (UV531), tris(1,2,2,6,6-pentamethylpiperidinol)phosphite (GW-540), and benzotriazole ultraviolet light absorber (UV327). The ultraviolet light absorber can absorb and filter out ultraviolet light of 280-400nm to improve the problem of easy light aging of the composite material and extend the service life of the composite material.

[0049] In some embodiments, the ultraviolet light absorber includes 2-hydroxy-4-n-octyloxybenzophenone, tris(1,2,2,6,6-pentamethylpiperidinol)phosphite and benzotriazole ultraviolet light absorber in a mass ratio of (0.8-1.2):(0.8-1.2):(0.8-1.2). The mass ratio of the above three ultraviolet light absorbers can be 1:1:1, 0.8:1:1.2, 1:0.8:1.2, 1.2:1:0.8, 0.8:1.2:1, etc., which is not specifically limited here.

[0050] Optionally, the antioxidant includes at least one of antioxidant 1010 and antioxidant 168. If the two are compounded, the weight ratio can be 1:1, 1:0.8, 0.9:1, etc., which is not specifically limited here. The antioxidant can improve the problem of thermal aging degradation of the composite material, so that when the composite material is used to prepare light diffusion devices such as lampshades, it has a longer service life and is not easily broken due to thermal aging.

[0051] The present disclosure also provides a method for preparing a light-diffusing polypropylene-polycarbonate composite material, comprising: mixing raw materials of the light-diffusing polypropylene-polycarbonate composite material and granulating. The preparation method is simple and easy to operate.

[0052] Optionally, the granulation may be performed by mixing, extruding and granulating the raw materials using a twin-screw extruder after the raw materials are mixed.

[0053] Optionally, the screw diameter is 30-40 mm; the aspect ratio is 40-44; the twin-screw extruder main engine speed is 250-500 r / min, the barrel temperature is 220-245°C, the water tank temperature is 20-60°C; the pelletizer speed is 400-700 r / min. The specific parameter selection of granulation is similar to the related technology and will not be repeated here.

[0054] The present invention is further described in detail below in conjunction with embodiments.

[0055] Example 1

[0056] The steps of preparing the light-diffusing polypropylene-polycarbonate composite material include:

[0057] (1) Weigh each component material in proportion, put it into a stirring pot and stir it evenly. The weight of each raw material is shown in Table 1.

[0058] Among them, the transmittance of homopolymer PP is 84%, the haze is 14%, the melt flow rate is 2g / 10min, and the refractive index is 1.45.

[0059] The light transmittance of the polycarbonate is 89%, the haze is 3%, the melt flow rate is 12 g / 10 min, and the refractive index is 1.57.

[0060] The maleic anhydride grafting rate of PP-g-MAH was 1.5%.

[0061] The mesh number of talcum powder is 5000 mesh, the whiteness is 95%, and the refractive index is 1.52.

[0062] The ultraviolet light absorber is a mixture of UV531, GW-540 and UV327 in a weight ratio of 1:1:1.

[0063] The antioxidants are antioxidants 1010 and 168 in a weight ratio of 1:1.

[0064] (2) adding the mixed material obtained in step (1) from the main feed port of a twin-screw extruder, mixing the mixed material evenly in the twin-screw extruder, and then extruding the mixed material, and pelletizing the mixed material in a pelletizer to obtain a light-diffusing polypropylene-polycarbonate composite material with a high adhesive effect.

[0065] Example 2

[0066] The difference between Example 2 and Example 1 is:

[0067] The ultraviolet light absorber is a mixture of UV531, GW-540 and UV327 in a weight ratio of 1:0.8:1.2.

[0068] For other process parameters, refer to Table 1 and Example 1.

[0069] Example 3

[0070] The difference between Example 3 and Example 1 is:

[0071] The ultraviolet light absorber is a mixture of UV531, GW-540 and UV327 in a weight ratio of 0.8:1.2:0.8.

[0072] For other process parameters, refer to Table 1 and Example 1.

[0073] Embodiment 4, 5

[0074] The differences between Examples 4 and 5 and Example 1 are shown in Table 1.

[0075] Example 6

[0076] The difference between Example 6 and Example 1 is that:

[0077] The transmittance of homopolymer PP is 85%, the haze is 10%, the melt flow rate is 1 g / 10 min, and the refractive index is 1.50.

[0078] The light transmittance of the polycarbonate is 90%, the haze is 5%, the melt flow rate is 10 g / 10 min, and the refractive index is 1.55.

[0079] The maleic anhydride grafting rate of PP-g-MAH was 1%.

[0080] The mesh number of talcum powder is 4500 mesh, the whiteness is 95%, and the refractive index is 1.51.

[0081] The antioxidant is antioxidant 1010.

[0082] Other process parameters refer to Example 1.

[0083] Example 7

[0084] The difference between Example 7 and Example 1 is that:

[0085] The transmittance of homopolymer PP is 80%, the haze is 16%, the melt flow rate is 3g / 10min, and the refractive index is 1.40.

[0086] The light transmittance of the polycarbonate is 86%, the haze is 1%, the melt flow rate is 15 g / 10 min, and the refractive index is 1.60.

[0087] The maleic anhydride grafting rate of PP-g-MAH was 2%.

[0088] The mesh number of talcum powder is 5500 mesh, the whiteness is 95%, and the refractive index is 1.53.

[0089] The antioxidant is antioxidant 168.

[0090] Other process parameters refer to Example 1.

[0091] Comparative Examples 1 and 2

[0092] The differences between Comparative Examples 1 and 2 and Example 1 are shown in Table 1.

[0093] Comparative Example 3

[0094] The difference between Comparative Example 3 and Example 1 is that the weight portion of polycarbonate PC is 0.5. The other process parameters are the same as those of Example 1.

[0095] Comparative Example 4

[0096] The difference between Comparative Example 4 and Example 1 is that the mesh number of the talc powder is 4000.

[0097] Other process parameters refer to Example 1.

[0098] Comparative Example 5

[0099] The difference between Comparative Example 5 and Example 1 is that the mesh number of the talc powder is 8000.

[0100] Other process parameters refer to Example 1.

[0101] Comparative Example 6

[0102] The difference between Comparative Example 6 and Example 1 is that no talc is added.

[0103] Other process parameters refer to Example 1.

[0104] Comparative Example 7

[0105] The difference between Comparative Example 7 and Example 1 is that the weight portion of talc is 2.

[0106] Other process parameters refer to Example 1.

[0107] Table 1

[0108]

[0109] Performance tests were conducted on each embodiment and comparative example, and the test contents included PC particle size in the composite material, light transmittance, ultraviolet light transmittance, tensile strength and impact strength of the composite material. Among them, the test method of PC particle size includes: after the composite material is brittle fractured with liquid nitrogen, scanning the cross section with an electron microscope to observe the PC particle size; light transmittance and haze can be most directly tested using optical performance testing equipment; the test method of ultraviolet light transmittance includes: testing the ultraviolet light passing through the composite material, after being absorbed, and passing through the diffuser plate to find the residual ultraviolet light; the test method of tensile strength and impact strength refers to conventional mechanical performance testing; the luminous flux is directly tested using an integrating sphere device; the beam angle is directly tested using a light distribution tester, and the test results are shown in Table 2.

[0110] Table 2

[0111]

[0112]

[0113] According to Table 2, when the percentage of PC to PP is between 1% and 5%, the composite material has both excellent optical and mechanical properties.

[0114] According to Comparative Examples 1 and 2, it can be seen that the appropriate amount of PC added can ensure good light transmittance, haze and mechanical properties of the composite material.

[0115] According to Comparative Example 3, the amount of PC added is too low to improve the haze, and the optical properties of the obtained material are poor.

[0116] According to Comparative Examples 4, 5, and 6, when the mesh size of talcum powder is too large or too small, or when no talcum powder is added, the haze cannot be improved, and the optical properties of the obtained material are poor.

[0117] According to Comparative Example 7, the amount of talcum powder added is too large, which reduces the light transmittance.

[0118] In summary, the light-diffusing polypropylene-polycarbonate composite material of the present invention can take into account both good optical properties and mechanical properties, and uses a small amount of PC as a light diffuser, breaking the inherent thinking of using diffusion powder to achieve light diffusion effect in related methods; and the preparation method is simple and easy to operate.

[0119] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A light diffusion polypropylene polycarbonate composite material, characterized in that: The raw materials of the light diffusion polypropylene polycarbonate composite material include, by weight: Homopolymer polypropylene 90-110 parts; 1-5 parts of polycarbonate; 3 to 6 parts of compatibilizer; 0.5-1 part of talcum powder; 0.2-0.4 parts of ultraviolet light absorber; Antioxidant 0.1-0.3 parts.

2. The light diffusion polypropylene polycarbonate composite material according to claim 1, characterized in that: The weight ratio of the polycarbonate to the homopolypropylene is 1% to 5%.

3. The light diffusion polypropylene polycarbonate composite material according to claim 2, characterized in that: The particle size of the polycarbonate in the light diffusion polypropylene polycarbonate composite material is 0.40 to 5.0 μm.

4. The light diffusion polypropylene polycarbonate composite material according to claim 1, characterized in that: The refractive index of the homopolypropylene is lower than that of the polycarbonate.

5. The light diffusion polypropylene polycarbonate composite material according to claim 4, characterized in that: The refractive index of the homopolypropylene is 1.40-1.50; the refractive index of the polycarbonate is 1.55-1.

60.

6. The light diffusion polypropylene polycarbonate composite material according to any one of claims 1 to 5, characterized in that: The light transmittance of the homopolypropylene is 80-85%, the haze of the homopolypropylene is 10-16%, and the melt flow rate of the homopolypropylene at a temperature of 230° C. is 1-3 g / 10 min; The light transmittance of the polycarbonate is 86-90%, the haze of the polycarbonate is 1-5%, and the melt flow rate of the polycarbonate at a temperature of 300° C. is 10-15 g / 10 min.

7. The light diffusion polypropylene polycarbonate composite material according to claim 1, characterized in that: The mesh number of the talc powder is 4500-5500 mesh, and the refractive index of the talc powder is 1.51-1.

53.

8. The light diffusion polypropylene polycarbonate composite material according to claim 1, characterized in that: The ultraviolet light absorber includes at least one of 2-hydroxy-4-n-octyloxybenzophenone, tris(1,2,2,6,6-pentamethylpiperidinol)phosphite and benzotriazole ultraviolet light absorber; and / or, The compatibilizer includes polypropylene grafted with maleic anhydride, wherein the grafting rate of maleic anhydride is 1-2%.

9. The light diffusion polypropylene polycarbonate composite material according to claim 8, characterized in that: The ultraviolet light absorber comprises the 2-hydroxy-4-n-octyloxybenzophenone, the tris(1,2,2,6,6-pentamethylpiperidinol)phosphite and the benzotriazole ultraviolet light absorber in a mass ratio of (0.8-1.2):(0.8-1.2):(0.8-1.2).

10. The method for preparing the light diffusion polypropylene polycarbonate composite material according to any one of claims 1 to 9, characterized in that: include: The raw materials of the light diffusion polypropylene polycarbonate composite material are mixed and granulated.