Optical glass
By reasonably adjusting the proportion of components such as P2O5, Nb2O5, TiO2, Na2O and K2O in optical glass, the refractive index and dispersion of optical glass are improved, and its secondary pressure-type crystallization resistance is significantly improved, solving the existing optical glass. The problem of insufficient anti-crystallation performance of glass in precision molding meets the needs of high-fine optical instruments.
Patent Information
- Application Number
- CN202411158160.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
AI Technical Summary
The existing optical glass has poor crystallization resistance during precision molding, resulting in a decrease in the quality of optical glass or scrapping, making it difficult to meet the needs of high refractive index and high dispersion.
Optical glass with specific component ratios is adopted, which contains P2O5, Nb2O5, TiO2, Na2O and K2O, and the TiO2/K2O ratio is 1.0-18.0, and P2O5/Nb2O5 is 0.4-0.85. The refractive index and dispersion are improved through reasonable component design. At the same time, the secondary pressurized crystallization resistance is optimized.
Optical glass with high refractive index and high dispersion have excellent secondary pressure crystallization resistance, improve the quality and stability of optical glass, and is suitable for the manufacturing of high-fine optical instruments.
Smart Images

Figure BDA0005005663290000161 
Figure BDA0005005663290000171 
Figure BDA0005005663290000172
Abstract
Description
Technical Field
[0001] The invention relates to optical glass, in particular to optical glass with excellent anti-crystallization performance. Background Art
[0002] In recent years, with the continuous integration of optics, electronic information science and new materials science, the application of optical glass as the basic material of optoelectronics in technical fields such as light transmission, light storage and optoelectronic display has developed rapidly. Optical instruments have developed rapidly in digitalization, integration and high precision, which puts higher requirements on the performance of optical glass used in optical instruments and equipment. Under the same radius of curvature, the higher the refractive index of the glass, the larger the imaging field of view, which is conducive to reducing the number of optical elements in optical instruments. With the development trend of miniaturization of optical instruments, the demand for high refractive index glass is becoming more and more obvious.
[0003] At present, the mainstream method of manufacturing optical glass into optical components is precision molding (including direct molding and secondary molding). The use of precision molding technology to manufacture optical components reduces the consumption of raw materials, reduces the cost of manpower and material resources, and reduces environmental pollution. This technology can produce optical components in large quantities at low cost. The so-called precision molding is to mold glass preforms with high-precision molds with a predetermined product shape under a certain temperature and pressure to obtain glass products with the final product shape and optical functions. Various optical glass products such as spherical lenses, aspherical lenses, prisms and diffraction gratings can be manufactured through precision molding technology. If the anti-crystallization performance of the optical glass is poor, crystallization is likely to occur in the optical glass during the process of manufacturing optical components by the precision molding method, resulting in a decline in the quality of the optical glass or even scrapping. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an optical glass with excellent secondary pressing anti-crystallization performance.
[0005] The technical solution adopted by the present invention to solve the technical problem is:
[0006] (1) Optical glass, the components of which, expressed in weight percentage, contain: P2O5: 20-34%; Nb2O5: 38-53%; TiO2: 8-22%; Na2O: 1-12%; K2O: greater than 0 but less than or equal to 10%, wherein TiO2 / K2O is 1.0-18.0.
[0007] (2) The optical glass according to (1), wherein the components, expressed in weight percentage, further contain: BaO: 0-8%; and / or CaO: 0-8%; and / or MgO: 0-5%; and / or SrO: 0-5%; and / or Li2O: 0-6%; and / or SiO2: 0-5%; and / or B2O3: 0-5%; and / or ZrO2: 0-5%; and / or Al2O3: 0-5%; and / or ZnO: 0-5%; and / or WO3: 0-5%; and / or Ln2O3: 0-5%; and / or Bi2O3: 0-5%; and / or a clarifier: 0-1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
[0008] (3) Optical glass, wherein the components include P2O5, Nb2O5, TiO2, Na2O and K2O, wherein the components are expressed in weight percentage, wherein TiO2 / K2O is 1.0 to 18.0, and the refractive index of the optical glass is n d 1.895~1.945, Abbe number ν d It is 15.5~21.5.
[0009] (4) The optical glass according to (3), wherein the components, expressed in weight percentage, are: P2O5: 20-34%; and / or Nb2O5: 38-53%; and / or TiO2: 8-22%; and / or Na2O: 1-12%; and / or K2O: greater than 0 but less than or equal to 10%; and / or BaO: 0-8%; and / or CaO: 0-8%; and / or MgO: 0-5%; and / or SrO: 0-5%; and / or Li2O: 0-6%; and / or SiO2: 0 ~5%; and / or B2O3: 0~5%; and / or ZrO2: 0~5%; and / or Al2O3: 0~5%; and / or ZnO: 0~5%; and / or WO3: 0~5%; and / or Ln2O3: 0~5%; and / or Bi2O3: 0~5%; and / or clarifier: 0~1%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
[0010] (5) The optical glass according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, satisfy one or more of the following 11 conditions:
[0011] 1) TiO2 / K2O is 1.0 to 12.0, preferably TiO2 / K2O is 1.5 to 10.0, and more preferably TiO2 / K2O is 2.0 to 8.0;
[0012] 2) P2O5 / Nb2O5 is 0.4 to 0.85, preferably P2O5 / Nb2O5 is 0.45 to 0.8, more preferably P2O5 / Nb2O5 is 0.5 to 0.7, and further preferably P2O5 / Nb2O5 is 0.55 to 0.65;
[0013] 3) TiO2 / Nb2O5 is 0.2 to 0.55, preferably TiO2 / Nb2O5 is 0.2 to 0.5, and more preferably TiO2 / Nb2O5 is 0.25 to 0.45;
[0014] 4) (Nb2O5+Na2O+BaO) / TiO2 is 1.8 to 5.5, preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.0 to 5.0, and more preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.5 to 4.5;
[0015] 5) (TiO2+K2O) / (BaO+Na2O) is 1.6 to 12.0, preferably (TiO2+K2O) / (BaO+Na2O) is 2.0 to 10.0, more preferably (TiO2+K2O) / (BaO+Na2O) is 2.2 to 7.0, and further preferably (TiO2+K2O) / (BaO+Na2O) is 2.5 to 5.5;
[0016] 6) CaO / BaO is 0.1 to 10.0, preferably CaO / BaO is 0.2 to 7.0, more preferably CaO / BaO is 0.3 to 5.0, and further preferably CaO / BaO is 0.5 to 3.0;
[0017] 7) (B2O3+SiO2) / CaO is less than 2.8, preferably (B2O3+SiO2) / CaO is 0.1 to 2.0, more preferably (B2O3+SiO2) / CaO is 0.2 to 1.5, and further preferably (B2O3+SiO2) / CaO is 0.4 to 1.0;
[0018] 8) (BaO + SrO + MgO + ZnO + ZrO2) / Na2O is less than 1.0, preferably
[0019] (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is less than 0.8, more preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is 0.05 to 0.6, and further preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is 0.1 to 0.5;
[0020] 9) (BaO + WO3) / K2O is less than 1.5, preferably (BaO + WO3) / K2O is less than 1.0, more preferably (BaO + WO3) / K2O is 0.05 to 0.7, and further preferably (BaO + WO3) / K2O is 0.1 to 0.5;
[0021] 10) WO3 / CaO is 0.9 or less, preferably WO3 / CaO is 0.7 or less, more preferably WO3 / CaO is 0.5 or less, and further preferably WO3 / CaO is 0.3 or less;
[0022] 11) (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 1.7 or less, preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 1.0 or less, more preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 0.7 or less, and further preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) /
[0023] (BaO+CaO) is 0.1-0.6, and the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3.
[0024] (6) The optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: P2O5: 22-32%, preferably P2O5: 25-29%; and / or Nb2O5: 40-50%, preferably Nb2O5: 42-47%; and / or TiO2: 11-20%, preferably TiO2: 13-18%; and / or Na2O: 2-10%, preferably Na2O: 3-8%; and / or K2O: 0.5-8%, preferably K2O: 1-6%; and / or BaO: greater than 0 but less than or equal to 6%, preferably BaO: 0.1-3.5%; and / or CaO: 0-6%, preferably CaO: 0.1-4%; and / or MgO: 0-3%, preferably MgO: 0-1%, more preferably MgO is not contained; and / or SrO: 0-3%, preferably SrO: 0-1%, more preferably SrO is not contained; and / or Li2O: 0-4%, preferably Li2O: 0-2%, more preferably Li2O is not contained; and / or SiO2: 0-3%, preferably SrO: 0-1%, more preferably SrO is not contained; iO2: 0-1%; and / or B2O3: 0-3%, preferably B2O3: 0-1.5%; and / or ZrO2: 0-3%, preferably ZrO2: 0-1%, more preferably no ZrO2; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%, more preferably no Al2O3; and / or ZnO: 0-3%, preferably ZnO: 0-1%, more preferably no ZnO; and / or WO3: 0-3%, preferably WO3: 0-1%, more preferably no WO 3; and / or Ln2O3: 0-3%, preferably Ln2O3: 0-1%, more preferably no Ln2O3; and / or Bi2O3: 0-3%, preferably Bi2O3: 0-1%, more preferably no Bi2O3; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
[0025] (7) The refractive index n of the optical glass according to any one of (1) to (4) d is 1.895 to 1.945, preferably 1.90 to 1.945, more preferably 1.91 to 1.94, and further preferably 1.915 to 1.93; Abbe number ν d It is 15.5 to 21.5, preferably 16 to 21, more preferably 17 to 20, and further preferably 17.5 to 19.5.
[0026] (8) The thermal expansion coefficient α of the optical glass according to any one of (1) to (4) 100 / 300℃ 100×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less; and / or acid resistance stability D A 2 or more, preferably 1; and / or water resistance stability D W Two or more types, preferably one type; and / or a transition temperature T g 680°C or less, preferably 670°C or less, more preferably 665°C or less, and further preferably 660°C or less; and / or abrasion degree F A is 160 to 220, preferably 170 to 210, more preferably 180 to 200; and / or density ρ is 3.80 g / cm 3 Below, preferably 3.70g / cm 3 Below, more preferably 3.60g / cm 3 Below, more preferably 3.50 g / cm 3 Below; and / or 70 450nm or less, preferably λ 70 445nm or less, more preferably λ 70 is 440nm or less; and / or the weather resistance CR is 2 or more, preferably 1; and / or the Young's modulus E is 9000×10 7 Pa or more, preferably 9500×10 7 Pa or more, more preferably 9800×10 7 Pa or more, more preferably 10000×10 7 Pa~11000×10 7 Pa; and / or the bubble degree is A grade or above, preferably A0 grade or above, more preferably A 00 and / or the stripe degree is C level or above, preferably B level or above; and / or the secondary pressing anti-crystallization performance is C level or above, preferably B level or above, more preferably A level.
[0027] (9) A glass preform made of the optical glass described in any one of (1) to (8).
[0028] (10) An optical element, made of the optical glass described in any one of (1) to (8), or made of the glass preform described in (9).
[0029] (11) An optical instrument comprising the optical glass described in any one of (1) to (8), or the optical element described in (10).
[0030] The beneficial effect of the present invention is that, through reasonable component design, the optical glass of the present invention has high refraction and high dispersion as well as excellent secondary compression molding anti-crystallization performance. DETAILED DESCRIPTION
[0031] The following will describe the embodiments of the optical glass of the present invention in detail, but the present invention is not limited to the following embodiments, and can be implemented by appropriate changes within the scope of the purpose of the present invention. In addition, although there are appropriate omissions of descriptions of the repeated descriptions, the gist of the invention will not be limited thereby, and in the following content, the optical glass of the present invention is sometimes referred to as glass.
[0032] [Optical glass]
[0033] The following is an explanation of the range of each component (ingredient) of the optical glass of the present invention. In the present invention, unless otherwise specified, the content, total content, and total content of each component are all expressed in weight percentage (wt%), that is, the content, total content, and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts, hydroxides, etc. used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.
[0034] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0035] <Essential Components and Optional Components>
[0036] P2O5 is a network generator of the glass of the present invention. Compared with silicate glass, phosphate glass can be melted at low temperature, which is beneficial to improve the light transmittance of the glass. If the content of P2O5 is too high, the viscosity-temperature curve of the glass in the forming area will become flatter, resulting in a slower cooling and solidification process during glass forming, which is very unfavorable for large-size glass forming. In addition, high content of P2O5 is easy to volatilize, which is not conducive to the glass obtaining a better stripe degree. Therefore, the content of P2O5 in the present invention is 20-34%, preferably 22-32%, and more preferably 25-29%. In some embodiments, the content of P2O5 may be 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%.
[0037] Nb2O5 is a high-refractive and high-dispersion component that can improve the refractive index and chemical stability of the glass. In the present invention, the above effect is obtained by containing more than 38% Nb2O5. Preferably, the content of Nb2O5 is more than 40%, and more preferably more than 42%. If the content of Nb2O5 is too high, the anti-crystallization performance of the glass decreases and the density increases. Therefore, in the present invention, the upper limit of the content of Nb2O5 is 53%, preferably 50%, and more preferably 47%. In some embodiments, the content of Nb2O5 may be 38%, 38.5%, 39%, 39.5%, 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5%, 50%, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%.
[0038] In some embodiments, the ratio of the content of P2O5 to the content of Nb2O5, P2O5 / Nb2O5, is controlled within the range of 0.4 to 0.85, so that the glass can more easily obtain the desired optical constants, and the thermal expansion coefficient of the glass can be reduced while optimizing the bubble degree of the glass. Therefore, preferably P2O5 / Nb2O5 is 0.4 to 0.85, more preferably P2O5 / Nb2O5 is 0.45 to 0.8, further preferably P2O5 / Nb2O5 is 0.5 to 0.7, and further preferably P2O5 / Nb2O5 is 0.55 to 0.65. In some embodiments, the value of P2O5 / Nb2O5 can be 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.6, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.7, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.8, 0.81, 0.82, 0.83, 0.84, 0.85.
[0039] TiO2 has the effect of increasing the refractive index and dispersion of glass and improving the resistance to devitrification. The present invention contains a suitable amount of TiO2 to make the glass more stable and reduce the high-temperature viscosity of the glass. The present invention obtains the above-mentioned effect by containing more than 8% TiO2, preferably more than 11% TiO2, and more preferably more than 13% TiO2. If the TiO2 content exceeds 22%, the crystallization tendency and coloring tendency of the glass increase, and the transition temperature rises. Therefore, the content of TiO2 in the present invention is less than 22%, preferably less than 20%, and more preferably less than 18%. In some embodiments, the TiO2 content may be 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%.
[0040] In some embodiments, the ratio of TiO2 to Nb2O5 is controlled within the range of 0.2 to 0.55, which can improve the weather resistance and Young's modulus of the glass while preventing the transmittance of the glass from decreasing. Therefore, preferably TiO2 / Nb2O5 is 0.2 to 0.55, more preferably TiO2 / Nb2O5 is 0.2 to 0.5, and further preferably TiO2 / Nb2O5 is 0.25 to 0.45. In some embodiments, the value of TiO2 / Nb2O5 may be 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.5, 0.51, 0.52, 0.53, 0.54, 0.55.
[0041] Na2O has the effect of improving the glass's solubility and light transmittance, and can also reduce the glass's transition temperature. If the Na2O content is too high, the glass's chemical stability and weather resistance will be reduced. Therefore, the Na2O content is 1 to 12%, preferably 2 to 10%, and more preferably 3 to 8%. In some embodiments, the Na2O content may be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%.
[0042] K2O has the effect of improving the devitrification resistance and melting property of glass. If its content is too high, it is difficult for the glass to obtain the desired high refractive index and high dispersion performance. Therefore, the content of K2O is greater than 0 but less than or equal to 10%, preferably 0.5-8%, and more preferably 1-6%. In some embodiments, the content of K2O may be greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%.
[0043] In some embodiments, the ratio of TiO2 to K2O is controlled within the range of 1.0 to 18.0, which can improve the weather resistance and secondary compression molding anti-crystallization performance of the glass. Therefore, preferably TiO2 / K2O is 1.0 to 18.0, and more preferably TiO2 / K2O is 1.0 to 12.0. Furthermore, the Young's modulus of the glass can be further optimized by making TiO2 / K2O within the range of 1.5 to 10.0. Therefore, it is further preferred that TiO2 / K2O is 1.5 to 10.0, and it is further preferred that TiO2 / K2O is 2.0 to 8.0. In some embodiments, the value of TiO2 / K2O may be 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0, 15.5, 16.0, 16.5, 17.0, 17.5, 18.0.
[0044] Li2O can reduce the transition temperature of glass, but its high content is not good for the acid resistance stability and thermal expansion coefficient of glass, and there is corrosion for melting containers (such as platinum crucibles). Therefore, the content of Li2O is 6% or less, preferably 4% or less, and more preferably 2% or less. In some embodiments, it is further preferred that Li2O is not contained. In some embodiments, the content of Li2O may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%.
[0045] BaO can improve the devitrification resistance and light transmittance of the glass in the present invention, and improve the secondary compression molding anti-crystallization performance of the glass. If the BaO content is too high, the chemical stability of the glass will deteriorate and the density will increase. Therefore, the BaO content is 0 to 8%, preferably greater than 0 but less than or equal to 6%, and more preferably 0.1 to 3.5%. In some embodiments, the BaO content can be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%.
[0046] In some embodiments, the ratio (Nb2O5+Na2O+BaO) / TiO2 between the total content of Nb2O5, Na2O, and BaO and the content of TiO2 is controlled within the range of 1.8 to 5.5, which can improve the bubble degree and striae degree of the glass and prevent the increase of the thermal expansion coefficient. Therefore, it is preferred that (Nb2O5+Na2O+BaO) / TiO2 is 1.8 to 5.5, more preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.0 to 5.0, and further preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.5 to 4.5. In some embodiments, the value of (Nb2O5+Na2O+BaO) / TiO2 may be 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5.
[0047] In some embodiments, the ratio (TiO2+K2O) / (BaO+Na2O) between the total content of TiO2 and K2O TiO2+K2O and the total content of BaO and Na2O BaO+Na2O is controlled within the range of 1.6 to 12.0, which can reduce the thermal expansion coefficient of the glass and increase the bubble degree of the glass. Therefore, it is preferred that (TiO2+K2O) / (BaO+Na2O) is 1.6 to 12.0, and it is more preferred that (TiO2+K2O) / (BaO+Na2O) is 2.0 to 10.0. Furthermore, by controlling (TiO2+K2O) / (BaO+Na2O) within the range of 2.2 to 7.0, the abrasiveness of the glass can be further optimized. Therefore, it is further preferred that (TiO2+K2O) / (BaO+Na2O) is 2.0 to 10.0.
[0048] (BaO+Na2O) is 2.2 to 7.0, and more preferably (TiO2+K2O) / (BaO+Na2O) is 2.5 to 5.5. In some embodiments, the value of (TiO2+K2O) / (BaO+Na2O) may be 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0.
[0049] SrO can improve the resistance of glass to devitrification and improve the melting performance of glass, but if its content is too high, the refractive index of the glass will be difficult to meet the design requirements, and the cost of the glass will also rise rapidly. Therefore, the content of SrO is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that SrO is not contained. In some embodiments, the content of SrO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0050] CaO helps to improve the light transmittance and density of the glass, but when the content of CaO is too much, it will make it difficult for the optical constants of the glass to meet the design requirements, and the anti-crystallization performance will deteriorate. Therefore, the content of CaO is 0-8%, preferably 0-6%, and more preferably 0.1-4%. In some embodiments, the content of CaO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%.
[0051] In some embodiments, the ratio of CaO content to BaO content CaO / BaO is controlled within the range of 0.1 to 10.0, which can reduce the density of the glass while improving the chemical stability and secondary compression molding anti-crystallization performance of the glass. Therefore, preferably CaO / BaO is 0.1 to 10.0, more preferably CaO / BaO is 0.2 to 7.0, further preferably CaO / BaO is 0.3 to 5.0, and further preferably CaO / BaO is 0.5 to 3.0. In some embodiments, the value of CaO / BaO can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0.
[0052] MgO can reduce the relative partial dispersion of glass, but when the MgO content is too high, the refractive index of the glass is difficult to meet the design requirements, and the anti-crystallization performance and stability of the glass are reduced. Therefore, the content of MgO is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that MgO is not contained. In some embodiments, the content of MgO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0053] SiO2 is beneficial to increase the molding viscosity of the glass, improve the striation degree of the glass, and is beneficial to use a quartz crucible to prepare clinker to avoid platinum contamination, thereby improving the transmittance of the glass. However, too high a SiO2 content will increase the glass melting temperature and the glass transition temperature. Therefore, the content of SiO2 is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%. In some embodiments, the content of SiO2 may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0054] B2O3 can improve the stability and solubility of glass. If its content is too high, the refractive index of the glass will decrease and the secondary compression molding anti-crystallization performance will deteriorate. Therefore, the content of B2O3 in the present invention is less than 5%, preferably less than 3%, and more preferably less than 1.5%. In some embodiments, the content of B2O3 may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0055] In some embodiments, the ratio (B2O3+SiO2) / CaO between the total content of B2O3 and SiO2 (B2O3+SiO2) and the content of CaO is controlled to be below 2.8, which can improve the striation degree of the glass and prevent the secondary compression molding anti-crystallization performance of the glass from decreasing. Therefore, it is preferred that (B2O3+SiO2) / CaO is below 2.8, and it is more preferred that (B2O3+SiO2) / CaO is 0.1 to 2.0. Furthermore, by controlling (B2O3+SiO2) / CaO within the range of 0.2 to 1.5, the weather resistance and coloring of the glass can be further optimized. Therefore, it is further preferred that (B2O3+SiO2) / CaO is 0.2 to 1.5, and it is further preferred that (B2O3+SiO2) / CaO is 0.4 to 1.0. In some embodiments, the value of (BO3+SiO2) / CaO can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8.
[0056] ZrO2 can increase the refractive index of glass and adjust dispersion, improve the anti-crystallization performance and strength of glass. If the ZrO2 content is too high, the difficulty of melting the glass will increase, the melting temperature will rise, and even inclusions will appear inside the glass and the transmittance will decrease. Therefore, the ZrO2 content is less than 5%, preferably 3%, and more preferably less than 1%. In some embodiments, it is further preferred that ZrO2 is not contained. In some embodiments, the ZrO2 content may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0057] Al2O3 can improve the chemical stability of glass, but when its content exceeds 5%, the solubility and light transmittance of the glass deteriorate. Therefore, the content of Al2O3 in the present invention is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Al2O3 is not contained. In some embodiments, the content of Al2O3 may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0058] ZnO can lower the transition temperature of glass, improve the chemical stability of glass, and reduce the high temperature viscosity of glass. If the ZnO content is too high, the anti-crystallization performance of the glass will deteriorate, and devitrification will easily occur due to the low viscosity. Therefore, the content of ZnO in the present invention is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that ZnO is not contained. In some embodiments, the content of ZnO may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0059] In some embodiments, the ratio of the total content of BaO, SrO, MgO, ZnO, and ZrO2, BaO+SrO+MgO+ZnO+ZrO2, to the content of Na2O, (BaO+SrO+MgO+ZnO+ZrO2) / Na2O, is controlled to be below 1.0, which can increase the striation degree of the glass and improve the abrasiveness of the glass. Therefore, it is preferred that (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is below 1.0, and more preferably
[0060] (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is less than 0.8, more preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is 0.05 to 0.6, and even more preferably (BaO+SrO+MgO+ZnO+ZrO2) / Na2O is 0.1 to 0.5. In some embodiments,
[0061] The value of (BaO+SrO+MgO+ZnO+ZrO2) / Na2O can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, and 1.0.
[0062] WO3 can improve the refractive index and dispersion of glass. If its content is too high, the light transmittance of the glass will decrease, and the secondary pressing anti-crystallization performance will deteriorate. Therefore, the content of WO3 is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that WO3 is not contained. In some embodiments, the content of WO3 may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0063] In some embodiments, the ratio (BaO+WO3) / K2O between the total content of BaO and WO3 BaO+WO3 and the content of K2O is controlled to be below 1.5, which can reduce the density of the glass and prevent the transition temperature of the glass from increasing. Therefore, it is preferred that (BaO+WO3) / K2O is below 1.5, and it is more preferred that (BaO+WO3) / K2O is below 1.0. Furthermore, by controlling (BaO+WO3) / K2O within the range of 0.05 to 0.7, the striation degree and Young's modulus of the glass can be further optimized. Therefore, it is further preferred that (BaO+WO3) / K2O is 0.05 to 0.7, and it is further preferred that (BaO+WO3) / K2O is 0.1 to 0.5. In some embodiments, the value of (BaO + WO3) / K2O can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5.
[0064] In some embodiments, the ratio of WO3 to CaO is controlled to be below 0.9, which can improve the anti-devitrification and chemical stability of the glass. Therefore, WO3 / CaO is preferably below 0.9, more preferably below 0.7, further preferably below 0.5, and further preferably below 0.3. In some embodiments, the value of WO3 / CaO can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9.
[0065] Ln2O3 (Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3) is a component that increases the refractive index and chemical stability of glass. By controlling the content of Ln2O3 to less than 5%, the devitrification resistance of glass can be prevented from decreasing. Preferably, the upper limit of the Ln2O3 content is 3%, and more preferably the upper limit is 1%. In some embodiments, it is further preferred that Ln2O3 is not contained. In some embodiments, the content of Ln2O3 may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%.
[0066] Bi2O3 can improve the water resistance of glass and reduce the transition temperature, but if its content is too high, the light transmittance of the glass will decrease, the abrasion resistance and chemical stability will deteriorate, and the density will increase significantly. Therefore, the content of Bi2O3 is 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Bi2O3 is not contained. In some embodiments, the content of Bi2O3 may be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0067] In some embodiments, the ratio of the total content of B2O3, SiO2, Al2O3, WO3, ZnO, ZrO2, Ln2O3, and Bi2O3 to the total content of BaO and CaO BaO+CaO (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is controlled below 1.7, which can improve the striae of the glass and optimize the abrasion resistance of the glass. Therefore, it is preferred that (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 1.7 or less, and it is more preferred that (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 1.0 or less, and it is further preferred that (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 0.7 or less, and it is further preferred that (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 0.1 to 0.6. In some embodiments,
[0068] The value of (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) can be 0, greater than 0, 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, and 1.7.
[0069] In the present invention, by containing 0-1% of one or more components of Sb2O3, SnO2, SnO, and CeO2 as a clarifier, the clarification effect of the glass can be improved and the bubble degree of the glass can be improved. Preferably, the content of the clarifier is 0-0.5%, and more preferably, the content of the clarifier is 0-0.1%. Since the component types and contents of the optical glass of the present invention are reasonably designed and its bubble degree is excellent, it is further preferred in some embodiments that no clarifier is contained. In some embodiments, the content of the clarifier can be 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%.
[0070] <Components that should not be contained>
[0071] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.
[0072] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are not actually contained except for being inevitably mixed in. Thus, the optical glass does not actually contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can be manufactured, processed and discarded.
[0073] In order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As2O3 and PbO.
[0074] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.
[0075] Next, the properties of the optical glass of the present invention will be described.
[0076] <Refractive Index and Abbe Number>
[0077] The refractive index of optical glass (n d) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.
[0078] In some embodiments, the refractive index (n d ) has a lower limit of 1.895, a preferred lower limit is 1.90, a more preferred lower limit is 1.91, and a further preferred lower limit is 1.915.
[0079] In some embodiments, the refractive index (n d ) is 1.945, preferably 1.94, and more preferably 1.93.
[0080] In some embodiments, the Abbe number (ν d ) has a lower limit of 15.5, a preferred lower limit of 16, a more preferred lower limit of 17, and a further preferred lower limit of 17.5.
[0081] In some embodiments, the Abbe number (ν d ) has an upper limit of 21.5, a preferred upper limit of 21, a more preferred upper limit of 20, and a further preferred upper limit of 19.5.
[0082] <Coefficient of Thermal Expansion>
[0083] Thermal expansion coefficient of optical glass (α 100 / 300℃ ) The data at 100-300℃ were tested according to the method specified in GB / T7962.16-2010.
[0084] In some embodiments, the thermal expansion coefficient (α 100 / 300℃ ) is 100×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less.
[0085] <Acid resistance stability>
[0086] Acid resistance stability of optical glass (D A ) (Powder method) Tested in accordance with the method specified in GB / T 17129.
[0087] In some embodiments, the acid resistance stability (D A ) is 2 or more types, preferably 1 type.
[0088] <Water resistance stability>
[0089] Water resistance stability of optical glass (D W) (Powder method) Tested in accordance with the method specified in GB / T 17129.
[0090] In some embodiments, the water resistance stability (D W ) is 2 or more types, preferably 1 type.
[0091] <Transition Temperature>
[0092] Transition temperature of optical glass (T g ) Tested according to the method specified in GB / T7962.16-2010.
[0093] In some embodiments, the transition temperature (T g ) is 680°C or lower, preferably 670°C or lower, more preferably 665°C or lower, and further preferably 660°C or lower.
[0094] <Abrasion>
[0095] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:
[0096]
[0097] Where: V—volume wear of the sample being tested;
[0098] V0—Volume loss of standard sample;
[0099] W—mass wear loss of the sample being tested;
[0100] W0—standard sample mass wear;
[0101] ρ—density of the sample being tested;
[0102] ρ0—standard sample density.
[0103] In some embodiments, the abrasiveness (F A ) has a lower limit of 160, a preferred lower limit of 170, and a more preferred lower limit of 180.
[0104] In some embodiments, the abrasiveness (F A ) has an upper limit of 220, a preferred upper limit of 210, and a more preferred upper limit of 200.
[0105] <density>
[0106] The density (ρ) is tested according to the method specified in GB / T7962.20-2010.
[0107] In some embodiments, the density (ρ) of the optical glass of the present invention is 3.80 g / cm 3 Below, preferably 3.70g / cm 3 Below, more preferably 3.60g / cm 3 Below, more preferably 3.50 g / cm 3 the following.
[0108] <Color>
[0109] The short-wave transmission spectrum characteristics of the glass of the present invention are expressed by the coloration (λ 70 ) indicates. 70 Refers to the wavelength when the glass transmittance reaches 70%. 70 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 70%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I in The amount expressed by λ also includes the transmittance of the surface reflection loss on the above surfaces of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, in high refractive index glass, λ 70 A small value of means that the glass itself is less colored and has a high light transmittance.
[0110] In some embodiments, the λ of the optical glass of the present invention is 70 450nm or less, preferably λ 70 445nm or less, more preferably λ 70 Below 440nm.
[0111] <Weather resistance>
[0112] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test box with a saturated water vapor environment of 90% relative humidity, alternately cycle every 1 hour at 40-50°C, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:
[0113] Table 1.
[0114]
[0115] In some embodiments, the weather resistance (CR) of the optical glass of the present invention is Class 2 or higher, preferably Class 1.
[0116] <Young's modulus>
[0117] Young's modulus (E) is calculated using the following formula by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity.
[0118]
[0119] G=V S 2 ρ
[0120] Where: E is Young's modulus, Pa;
[0121] G is the shear modulus, Pa;
[0122] V T is the shear wave velocity, m / s;
[0123] V S is the longitudinal wave velocity, m / s;
[0124] ρ is the glass density, g / cm 3 .
[0125] In some embodiments, the Young's modulus (E) of the optical glass of the present invention is 9000×10 7 Pa or more, preferably 9500×10 7 Pa or more, more preferably 9800×10 7 Pa or more, more preferably 10000×10 7 Pa~11000×10 7 Pa.
[0126] <Bubble Degree>
[0127] The bubble degree of optical glass is tested according to the method specified in GB / T7962.8-2010.
[0128] In some embodiments, the bubble degree of the optical glass of the present invention is above grade A, preferably above grade A0, and more preferably above grade A1. 00 class.
[0129] <Striation Degree>
[0130] The striation degree of the glass of the present invention is tested by the following method: using a striation meter composed of a point light source and a lens, the striation degree is compared with the standard sample from the direction where the striation is most easily visible, and is divided into 4 levels, namely, A, B, C, and D. Level A means no striations visible to the naked eye under the specified test conditions, level B means fine and dispersed striations under the specified test conditions, level C means slight parallel striations under the specified test conditions, and level D means coarse striations under the specified test conditions.
[0131] In some embodiments, the striae degree of the optical glass of the present invention is C level or higher, preferably B level or higher.
[0132] <Secondary Pressing Anti-Crystallization Performance>
[0133] The test method of the secondary pressing anti-crystallization performance is as follows: cut the sample glass into 20×20×10mm specifications and place it in a temperature of T g Keep the glass in a muffle furnace at +(200-250)℃ for 15-30 minutes (the present invention uses 880℃ for 15 minutes), take it out and cool it down, and observe whether there is devitrification or crystal particles on the surface and inside of the glass. If the glass sample has no devitrification and crystal particles, the secondary pressing anti-crystallization performance of the glass is excellent.
[0134] In the secondary pressing anti-crystallization performance test, according to the above-mentioned test method, the glass with no devitrification or crystallization grains on the surface and no crystal particles inside is recorded as "A", the glass with no crystallization grains inside but devitrification or crystallization grains on the surface is recorded as "B" (the devitrification or crystallization grains on the surface of the glass during the secondary pressing can be removed by grinding, but the grinding cost may increase), the glass with 1 to 10 crystal particles inside is recorded as "C", the glass with 10 to 20 crystal particles inside is recorded as "D", and the glass with more than 20 densely packed crystallization particles inside is recorded as "×".
[0135] In some embodiments, the secondary pressing anti-devitrification performance of the optical glass of the present invention is C level or above, preferably B level or above, and more preferably A level.
[0136] [Method for producing optical glass]
[0137] The manufacturing method of the optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, complex salts (such as carbonates, nitrates, sulfates, phosphates, metaphosphates, etc.), boric acid, etc. as raw materials, and after the ingredients are prepared according to the conventional method, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucible) at 1000-1300°C for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.
[0138] [Glass preforms and optical components]
[0139] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.
[0140] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.
[0141] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.
[0142] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.
[0143] [Optical instruments]
[0144] The optical element formed by the optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.
[0145] Example
[0146] <Optical Glass Example>
[0147] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.
[0148] This embodiment adopts the above optical glass manufacturing method to obtain optical glasses having the compositions shown in Tables 2 to 4. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 2 to 4.
[0149] Table 2.
[0150]
[0151]
[0152]
[0153] Table 3.
[0154]
[0155]
[0156] Table 4.
[0157]
[0158]
[0159]
[0160] <Glass Preform Example>
[0161] The glass obtained from optical glass examples 1 to 21# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.
[0162] <Optical Element Embodiment>
[0163] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the internal stress of the glass and fine-tune the refractive index so that the optical properties such as the refractive index reach the desired values.
[0164] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.
[0165] <Optical Instrument Embodiment>
[0166] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips.
Claims
1. Optical glass, characterized in that: Its components are expressed in weight percentage and contain: P2O5: 20-34%; Nb2O5: 38-53%; TiO2: 8-22%; Na2O: 1-12%; K2O: greater than 0 but less than or equal to 10%, wherein TiO2 / K2O is 1.0-18.
0.
2. The optical glass according to claim 1, characterized in that: Its components, expressed in weight percentage, also contain: BaO: 0-8%; and / or CaO: 0-8%; and / or MgO: 0-5%; and / or SrO: 0-5%; and / or Li2O: 0-6%; and / or SiO2: 0-5%; and / or B2O3: 0-5%; and / or ZrO2: 0-5%; and / or Al2O3: 0-5%; and / or ZnO: 0-5%; and / or WO3: 0-5%; and / or Ln2O3: 0-5%; and / or Bi2O3: 0-5%; and / or clarifier: 0-1%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
3. Optical glass, characterized in that: The components include P2O5, Nb2O5, TiO2, Na2O and K2O, and the components are expressed in weight percentage, wherein TiO2 / K2O is 1.0 to 18.0, and the refractive index of the optical glass is n d 1.895~1.945, Abbe number ν d It is 15.5~21.
5.
4. The optical glass according to claim 3, characterized in that: Its components, expressed in weight percentage, contain: P2O5: 20-34%; and / or Nb2O5: 38-53%; and / or TiO2: 8-22%; and / or Na2O: 1-12%; and / or K2O: greater than 0 but less than or equal to 10%; and / or BaO: 0-8%; and / or CaO: 0-8%; and / or MgO: 0-5%; and / or SrO: 0-5%; and / or Li2O: 0-6%; and / or SiO2: 0-5%; and / or B 2O3: 0-5%; and / or ZrO2: 0-5%; and / or Al2O3: 0-5%; and / or ZnO: 0-5%; and / or WO3: 0-5%; and / or Ln2O3: 0-5%; and / or Bi2O3: 0-5%; and / or clarifier: 0-1%, wherein Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
5. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following 11 conditions: 1) TiO2 / K2O is 1.0 to 12.0, preferably TiO2 / K2O is 1.5 to 10.0, and more preferably TiO2 / K2O is 2.0 to 8.0; 2) P2O5 / Nb2O5 is 0.4 to 0.85, preferably P2O5 / Nb2O5 is 0.45 to 0.8, more preferably P2O5 / Nb2O5 is 0.5 to 0.7, and further preferably P2O5 / Nb2O5 is 0.55 to 0.65; 3) TiO2 / Nb2O5 is 0.2 to 0.55, preferably TiO2 / Nb2O5 is 0.2 to 0.5, and more preferably TiO2 / Nb2O5 is 0.25 to 0.45; 4) (Nb2O5+Na2O+BaO) / TiO2 is 1.8 to 5.5, preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.0 to 5.0, and more preferably (Nb2O5+Na2O+BaO) / TiO2 is 2.5 to 4.5; 5) (TiO2+K2O) / (BaO+Na2O) is 1.6 to 12.0, preferably (TiO2+K2O) / (BaO+Na2O) is 2.0 to 10.0, more preferably (TiO2+K2O) / (BaO+Na2O) is 2.2 to 7.0, and further preferably (TiO2+K2O) / (BaO+Na2O) is 2.5 to 5.5; 6) CaO / BaO is 0.1 to 10.0, preferably CaO / BaO is 0.2 to 7.0, more preferably CaO / BaO is 0.3 to 5.0, and further preferably CaO / BaO is 0.5 to 3.0; 7) (B2O3+SiO2) / CaO is less than 2.8, preferably (B2O3+SiO2) / CaO is 0.1 to 2.0, more preferably (B2O3+SiO2) / CaO is 0.2 to 1.5, and further preferably (B2O3+SiO2) / CaO is 0.4 to 1.0; 8) (BaO + SrO + MgO + ZnO + ZrO2) / Na2O is less than 1.0, preferably (BaO + SrO + MgO + ZnO + ZrO2) / Na2O is less than 0.8, more preferably (BaO + SrO + MgO + ZnO + ZrO2) / Na2O is 0.05 to 0.6, and further preferably (BaO + SrO + MgO + ZnO + ZrO2) / Na2O is 0.1 to 0.5; 9) (BaO + WO3) / K2O is less than 1.5, preferably (BaO + WO3) / K2O is less than 1.0, more preferably (BaO + WO3) / K2O is 0.05 to 0.7, and further preferably (BaO + WO3) / K2O is 0.1 to 0.5; 10) WO3 / CaO is 0.9 or less, preferably WO3 / CaO is 0.7 or less, more preferably WO3 / CaO is 0.5 or less, and further preferably WO3 / CaO is 0.3 or less; 11) (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is less than 1.7, preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is less than 1.0, more preferably (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is less than 1.0 Preferably, (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is below 0.7, and further preferably, (B2O3+SiO2+Al2O3+WO3+ZnO+ZrO2+Ln2O3+Bi2O3) / (BaO+CaO) is 0.1-0.6, and the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3.
6. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: P2O5: 22-32%, preferably P2O5: 25-29%; and / or Nb2O5: 40-50%, preferably Nb2O5: 42-47%; and / or TiO2: 11-20%, preferably TiO2: 13-18%; and / or Na2O: 2-10%, preferably Na2O: 3-8%; and / or K2O: 0.5-8%, preferably K2O: 1-6%; and / or BaO: greater than 0 but less than or equal to 6% , preferably BaO: 0.1-3.5%; and / or CaO: 0-6%, preferably CaO: 0.1-4%; and / or MgO: 0-3%, preferably MgO: 0-1%, more preferably MgO is not contained; and / or SrO: 0-3%, preferably SrO: 0-1%, more preferably SrO is not contained; and / or Li2O: 0-4%, preferably Li2O: 0-2%, more preferably Li2O is not contained; and / or SiO2: 0-3%, preferably SiO2: 0-1%; and / or or B2O3: 0-3%, preferably B2O3: 0-1.5%; and / or ZrO2: 0-3%, preferably ZrO2: 0-1%, more preferably no ZrO2; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%, more preferably no Al2O3; and / or ZnO: 0-3%, preferably ZnO: 0-1%, more preferably no ZnO; and / or WO3: 0-3%, preferably WO3: 0-1%, more preferably no WO3; and / or L n2O3: 0-3%, preferably Ln2O3: 0-1%, more preferably no Ln2O3; and / or Bi2O3: 0-3%, preferably Bi2O3: 0-1%, more preferably no Bi2O3; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.1%, wherein the Ln2O3 is one or more of La2O3, Gd2O3, Y2O3, and Yb2O3, and the clarifier is one or more of Sb2O3, SnO2, SnO, and CeO2.
7. The optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the optical glass d is 1.895 to 1.945, preferably 1.90 to 1.945, more preferably 1.91 to 1.94, and further preferably 1.915 to 1.93; Abbe number ν d It is 15.5 to 21.5, preferably 16 to 21, more preferably 17 to 20, and further preferably 17.5 to 19.
5.
8. The optical glass according to any one of claims 1 to 4, characterized in that: The thermal expansion coefficient of the optical glass is α 100 / 300℃ 100×10 -7 / K or less, preferably 90×10 -7 / K or less, more preferably 85×10 -7 / K or less; and / or acid resistance stability D A 2 or more, preferably 1; and / or water resistance stability D W Two or more types, preferably one type; and / or a transition temperature T g 680°C or less, preferably 670°C or less, more preferably 665°C or less, and further preferably 660°C or less; and / or abrasion degree F A is 160 to 220, preferably 170 to 210, more preferably 180 to 200; and / or density ρ is 3.80 g / cm 3 Below, preferably 3.70g / cm 3 Below, more preferably 3.60g / cm 3 Below, more preferably 3.50 g / cm 3 Below; and / or 70 450nm or less, preferably λ 70 445nm or less, preferably λ 70 is 440nm or less; and / or the weather resistance CR is 2 or more, preferably 1; and / or the Young's modulus E is 9000×10 7 Pa or more, preferably 9500×10 7 Pa or more, more preferably 9800×10 7 Pa or more, more preferably 10000×10 7 Pa~11000×10 7 Pa; and / or the bubble degree is A grade or above, preferably A0 grade or above, more preferably A 00 and / or the stripe degree is C level or above, preferably B level or above; and / or the secondary pressing anti-crystallization performance is C level or above, preferably B level or above, more preferably A level.
9. A glass preform made of the optical glass according to any one of claims 1 to 8.
10. An optical element, made of the optical glass according to any one of claims 1 to 8, or made of the glass preform according to claim 9.
11. An optical instrument comprising the optical glass according to any one of claims 1 to 8, or the optical element according to claim 10.