A method for treating nickel-aluminum waste and separating nickel-aluminum
The microwave roasting process, which combines microwave short-time activation of nickel-aluminum waste pellets with molten flux, solves the problem of separating nickel and aluminum from nickel-aluminum waste, achieving efficient and low-cost resource recovery. It is suitable for the preparation of nickel-based catalysts.
Patent Information
- Application Number
- CN202410373584.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing technologies are insufficient for effectively separating and recovering nickel and aluminum from nickel-aluminum waste, especially the insoluble NiAl26O40 phase, resulting in high processing costs, high energy consumption, and high equipment requirements.
A microwave roasting process combining short-time microwave activation of nickel-aluminum scrap pellets with molten flux is employed. By leveraging the excellent microwave absorption and rapid heating characteristics of the flux under a microwave field, the Ni-Al-O chemical bonds are broken, achieving effective separation of nickel and aluminum.
It achieves rapid and effective separation of nickel and aluminum in nickel-aluminum waste, with an aluminum recovery rate of over 97% and a nickel leaching rate of less than 0.1%. The leaching solution has high purity, which simplifies the subsequent purification process and reduces production costs.
Smart Images

Figure HDA0004766346600000011 
Figure HDA0004766346600000012
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid waste resource recycling, and in particular to a method for treating nickel-aluminum waste to separate nickel-aluminum metals. Background Art
[0002] Nickel-aluminum alloy powder is an important raw material for preparing skeleton nickel catalysts. Nickel-aluminum alloy powder is treated with concentrated sodium hydroxide solution to form skeleton nickel catalysts with hydrogenation, dehydrogenation, deacidification, oxidation, methanation and other functions. It can be widely used in petrochemical, pharmaceutical, oil, fragrance, dye, synthetic fiber and other industrial fields. It has the advantages of high catalytic performance, low price, good thermal conductivity, high mechanical strength, and insensitivity to poisons.
[0003] Raney nickel catalyst is a solid heterogeneous catalyst composed of fine grains of nickel-aluminum alloy with a porous structure. It is obtained by activating nickel-aluminum alloy powder and is mainly used in catalytic hydrogenation reactions. After repeated use, the catalytic activity of Raney nickel catalyst decreases, and a large amount of waste nickel-aluminum powder is produced after deactivation. This waste nickel-aluminum powder is an important secondary resource. At present, when treating this waste nickel-aluminum powder, it is treated with strong alkali. Strong alkali solution can basically completely dissolve and remove the easily soluble aluminum in the waste nickel-aluminum powder. However, some difficult-to-treat phases produced during the use of the catalyst are difficult to dissolve, forming a slag phase after strong alkali treatment, that is, nickel-aluminum waste. Under the current severe reality of the decreasing mineral resources and the worsening ecological environment damage, conducting research on the comprehensive recovery and utilization of nickel and aluminum in nickel-aluminum waste has both environmental and economic benefits.
[0004] The present invention aims to provide a method for treating nickel-aluminum waste to separate nickel-aluminum metal therein, so as to achieve effective recovery of nickel-aluminum resources in the nickel-aluminum waste. Summary of the invention
[0005] The main technical problem solved by the present invention is to provide a method for treating nickel-aluminum waste and separating nickel and aluminum, which can realize the effective recovery of nickel and aluminum in the nickel-aluminum waste.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for treating nickel-aluminum waste to separate nickel and aluminum, comprising the steps of:
[0007] S1: forming nickel-aluminum waste into balls, and then performing short-time activation in a microwave environment to obtain activated nickel-aluminum waste balls; wherein the conditions for short-time activation are: microwave power of 300-500W, and calcination temperature of 350-450°C;
[0008] S2: mixing the activated nickel-aluminum waste balls with a molten flux, and roasting them in a microwave environment to obtain roasted slag; the roasting conditions are: microwave power 500-1000W, roasting temperature 550-750°C;
[0009] S3: treating the roasted slag by water leaching, and then performing solid-liquid separation to obtain an aluminum-containing leaching solution and a nickel-containing leaching slag.
[0010] As an implementation scheme of the present invention, the nickel-aluminum waste is mixed with water to form balls, and the ball diameter is controlled to be 1 to 2 cm.
[0011] As an embodiment of the present invention, the flux is sodium hydroxide and / or potassium hydroxide.
[0012] As an embodiment of the present invention, the molar number of the flux is 1.2 to 2.5 times the molar number of aluminum ions contained in the nickel-aluminum waste.
[0013] Preferably, the molar number of the flux is 1.8 to 2.1 times the molar number of aluminum ions contained in the nickel-aluminum waste.
[0014] As an embodiment of the present invention, the short-time activation time is controlled to be 1 to 3 minutes.
[0015] As an embodiment of the present invention, the melting of the flux is carried out in a microwave environment, and the melting conditions are: microwave power 300-500W, temperature 350-450°C, and time controlled to 5-8min.
[0016] As an embodiment of the present invention, in step S2, when roasting in a microwave environment, the roasting time is controlled to be 10 to 15 minutes.
[0017] As an embodiment of the present invention, in step S3, the water immersion treatment conditions are: leaching temperature 70-90° C., and treatment time 20-30 min.
[0018] As an embodiment of the present invention, before the calcined slag is treated by water immersion, water is first added to prepare a water-containing calcined slag material, and the liquid-to-solid ratio of the water-containing calcined slag material is 2.5-5.0 mL / g. The liquid-to-solid ratio refers to the ratio of the liquid volume (mL) of the water-containing calcined slag material to the mass (g) of the material contained. The water immersion treatment includes: heating the water-containing calcined slag material to 70-90°C and stirring for 20-30 minutes.
[0019] The aluminum-containing leaching solution obtained by the treatment of the present invention has an aluminum content of ≥98% by mass based on the total mass of the metals contained (excluding sodium or potassium), and the purity of the leaching solution is high.
[0020] The nickel-containing leaching residue obtained by the present invention has a nickel content of ≥99% by mass based on the total mass of the metals contained. The leaching residue can be directly used as a raw material for catalyst preparation after simple treatment.
[0021] The present invention provides a method for treating nickel-aluminum waste to separate nickel and aluminum. The raw material nickel-aluminum waste is solid waste residue after waste nickel-aluminum powder is treated with a strong alkali, and the easily soluble aluminum in the waste nickel-aluminum powder has been basically completely removed. 26 O 40 The method of the present invention can realize the recovery of insoluble NiAl in the difficult-to-treat nickel-aluminum waste. 26 O 40 The effective separation of nickel and aluminum in the physical phase greatly improves the separation efficiency of nickel and aluminum in difficult-to-treat nickel-aluminum waste. The nickel-containing leaching residue can be directly used as a raw material for the preparation of nickel-based catalysts after simple treatment.
[0022] Insoluble phase NiAl 26 O 40 The effective separation of nickel and aluminum is a difficult problem, because NiAl 26 O 40 The insoluble phase is a stable structure. The effective separation of nickel and aluminum can only be achieved under the premise that the chemical bonds are broken. This often requires harsh process conditions. The almost complete dissolution of aluminum can only be achieved under high temperature, high pressure and long time. The production cost is high, the energy consumption is large, and the equipment requirements are high.
[0023] The inventors found that the insoluble NiAl in nickel-aluminum waste 26 O 40The chemical bonds of the physical phases are stable and difficult to decompose under low temperature conditions. Only under high temperature conditions or special field conditions can the chemical bonds be destroyed. The present invention utilizes the special effect of microwaves on the Ni-Al-O chemical bonds and the excellent microwave absorption characteristics of the flux under the microwave field, and proposes a microwave roasting treatment process for nickel-aluminum waste pelletizing that combines microwave short-time activation with a molten flux. Microwave short-time and low-temperature activation of nickel-aluminum waste pelletizing utilizes the rapid heating property of microwaves on water, which macroscopically achieves rapid drying of water in the pellets, initially making the pellets present a loose and porous structure appearance, and microscopically promotes the initial destruction of the bond energy of the Ni-Al-O chemical bonds and enters an activated state; at the same time, pelletizing can avoid the problem of instantaneous agglomeration and wrapping when powdered raw materials are directly added to the molten flux under the microwave field. The molten state of the flux under the microwave field is the prerequisite for effective separation. This is because the selection of the flux is based on the results of multiple groups of microwave performance test experiments. The flux must have excellent microwave absorption characteristics. In the molten state, it can promote the effective chemical reaction contact between the subsequent raw materials (spherical) and the flux. Moreover, the rapid heating of the flux under the microwave field, if not in the molten state, will inevitably cause a temperature difference between the raw materials and the flux, which is not conducive to the stability of the subsequent reaction. The microwave roasting after the raw materials (spherical) contact with the molten flux appropriately increases the microwave power and temperature. Macroscopically, the high-power microwave field makes the loose and porous structure more obvious, providing conditions and channels for the deep destruction of microwaves. Microscopically, the Ni-Al-O chemical bond is destroyed. At the same time, the molten flux continues to deeply destroy the chemical bond, forming a synergistic effect, promoting the conversion of aluminum into soluble aluminates, and realizing the smooth progress of the subsequent leaching reaction.
[0024] The study also found that the short-time microwave activation and flux melting time for nickel-aluminum waste pelletizing should not be too long or too short. If the short-time microwave activation time of nickel-aluminum waste (spherical) is too short, it is not conducive to promoting the formation of a loose and porous structure of the pellets. If the time is too long, the temperature difference between the raw materials and water will easily increase the phenomenon of pellet powder falling off, which is not conducive to the subsequent contact reaction with the molten flux. If the flux melting time is too short, the melting is incomplete. If the time is too long, it is easy to cause overheating inside the flux, causing the internal chemical structure of the flux to change, which is not conducive to the subsequent roasting reaction with the nickel-aluminum waste balls. Therefore, it is very important to control the roasting time. Only by controlling the microwave roasting within the appropriate time range can NiAl be achieved. 26 O 40 Effective separation of nickel and aluminum in physical phases.
[0025] The invention is designed for the unique insoluble composition and structure characteristics of the raw material nickel-aluminum waste. Experiments show that the method of the invention can leach most of the aluminum in the nickel-aluminum waste, and the recovery rate of aluminum reaches more than 97%. At the same time, the leaching rate of nickel is lower than 0.1%. The obtained leaching solution has high purity, and the subsequent purification process of aluminum is greatly simplified. The nickel content (calculated by the total weight of metal) in the nickel-containing leaching residue after leaching is greater than 99%, and the purity is high. The leaching residue can be directly used as a raw material for preparing a nickel-based catalyst after simple treatment.
[0026] The method for separating nickel and aluminum from difficult-to-treat nickel-aluminum waste provided by the present invention realizes the rapid and effective separation of nickel and aluminum in difficult-to-treat nickel-aluminum waste, and the recycling method has low production cost, low labor intensity, short processing time, and increased processing capacity, which is more conducive to promoting the resource processing of nickel-aluminum waste and realizing energy conservation, emission reduction and green production in the nickel-aluminum industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The NiAl in the nickel-aluminum waste treated in Example 1 of the present invention 26 O 40 SEM image of the insoluble phase;
[0028] Figure 2 This is a picture of the roasted slag obtained by processing in step S2 in Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in detail below through specific embodiments. The following embodiments are intended to further illustrate the content of the present invention in detail, but are not intended to limit the scope of protection of the claims of the present invention.
[0030] In the following examples, the pharmaceutical agents used are all commercially available products. Unless otherwise specified, the content percentages in each example are all mass percentages.
[0031] Example 1
[0032] This embodiment provides a method for treating nickel-aluminum waste to separate nickel and aluminum. The raw material for treatment is provided by a chemical enterprise in Jiangxi Province. It is nickel-aluminum waste obtained by treating waste nickel-aluminum powder with strong alkali. The appearance is light green powder. The chemical composition analysis of its main valuable metals is shown in Table 1 below, where the content of each element is the mass percentage content. 26 O 40 The mass percentage of the insoluble phase is >98%, SEM NiAl 26 O 40 Phase diagram of sparingly soluble substances Figure 1 shown.
[0033] Table 1
[0034] element NiO <![CDATA[Al2O3]]> Content, Wt% 3.12 96.53
[0035] The processing steps are as follows:
[0036] S1: placing a flux sodium hydroxide in a crucible, the molar number of the flux is 1.8 times the molar number of aluminum ions contained in the nickel-aluminum waste, heating and heating the sodium hydroxide in a microwave roasting furnace to melt the sodium hydroxide, and the melting conditions are: microwave power 400W, roasting temperature 350°C, and time control 8min; after the flux is melted, a spherical material (the diameter of the ball is controlled to be 1-2cm) prepared by mixing the nickel-aluminum waste and water is placed in a spoon, inserted from the top of the microwave roasting furnace, and suspended in the microwave roasting furnace for short-term activation, and the conditions for short-term activation are: microwave power 400W, roasting temperature 350°C, and time control 3min;
[0037] S2: Slowly pour the short-time activated nickel-aluminum waste balls into the molten sodium hydroxide as a co-solvent, and roast them in a microwave roasting furnace to obtain roasted slag, see the photo Figure 2 ; The microwave roasting conditions were controlled as follows: microwave power 1000W, roasting temperature 750℃, and time control 10min;
[0038] S3: The calcined slag (spherical) is first added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 2.5 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 70° C., stirred for 25 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0039] After testing and analysis, most of the aluminum in the raw nickel-aluminum waste entered the leaching solution, the aluminum recovery rate was 98%, and the nickel leaching rate was 0.08%. Calculated by the total mass of metals in the leaching solution (excluding sodium), the mass fraction of aluminum was 98.89%, indicating that the main metal contained in the leaching solution was aluminum, and the purity was very high.
[0040] The mass percentage content of nickel in the leaching residue (calculated based on the total mass of metals contained in the leaching residue) is 99.2%.
[0041] Example 2
[0042] This embodiment provides a method for treating nickel-aluminum waste to separate nickel and aluminum, and the raw materials treated are the same as those in Example 1.
[0043] The processing steps are as follows:
[0044] S1: Potassium hydroxide as flux is placed in a crucible, the number of moles of the flux is 1.9 times the number of moles of aluminum ions contained in the nickel-aluminum waste, and the potassium hydroxide is melted by heating in a microwave roasting furnace, and the melting conditions are: microwave power 500W, roasting temperature 450°C, and time control 5min; after the flux is melted, a spherical material (the diameter of the ball is controlled to be 1-2cm) prepared by mixing the nickel-aluminum waste and water is placed in a spoon, inserted from the top of the microwave roasting furnace, and suspended in the microwave roasting furnace for short-term activation, and the conditions for short-term activation are: microwave power 500W, roasting temperature 450°C, and time control 2min;
[0045] S2: slowly pouring the short-time activated nickel-aluminum waste balls into the molten auxiliary solvent potassium hydroxide, and roasting them in a microwave roasting furnace to obtain roasted slag; the microwave roasting conditions are controlled as follows: microwave power 800W, roasting temperature 600℃, and time control 12min;
[0046] S3: The calcined slag (spherical) is first added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 3.0 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 80° C., stirred for 30 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0047] After testing and analysis, most of the aluminum in the raw nickel-aluminum waste entered the leaching solution, the aluminum recovery rate was 99%, and the nickel leaching rate was 0.05%. Calculated by the total mass of metals in the leaching solution (excluding potassium), the mass fraction of aluminum was 99.08%, indicating that the main metal contained in the leaching solution was aluminum, and the purity was very high.
[0048] The mass percentage content of nickel in the leaching residue (calculated based on the total mass of metals contained in the leaching residue) is 99.3%.
[0049] Example 3
[0050] This embodiment provides a method for treating nickel-aluminum waste to separate nickel and aluminum, and the raw materials treated are the same as those in Example 1.
[0051] The processing steps are as follows:
[0052] S1: Potassium hydroxide as flux is placed in a crucible, the number of moles of the flux is 2.0 times the number of moles of aluminum ions contained in the nickel-aluminum waste, and the potassium hydroxide is melted by heating in a microwave roasting furnace, and the melting conditions are: microwave power 300W, roasting temperature 400°C, and time control 6min; after the flux is melted, a spherical material (the diameter of the ball is controlled to be 1-2cm) prepared by mixing the nickel-aluminum waste and water is placed in a spoon, inserted from the top of the microwave roasting furnace, and hung in the microwave roasting furnace for short-term activation, and the conditions for short-term activation are: microwave power 300W, roasting temperature 400°C, and time control 1min;
[0053] S2: slowly pouring the short-time activated nickel-aluminum waste balls into the molten auxiliary solvent potassium hydroxide, and roasting them in a microwave roasting furnace to obtain roasted slag; the microwave roasting conditions are controlled as follows: microwave power 750W, roasting temperature 650℃, and time control 14min;
[0054] S3: The calcined slag (spherical) is first added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 4.0 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 80° C., stirred for 20 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0055] After testing and analysis, most of the aluminum in the raw nickel-aluminum waste entered the leaching solution, the aluminum recovery rate was 97%, and the nickel leaching rate was 0.06%. Calculated by the total mass of metals in the leaching solution (excluding potassium), the mass fraction of aluminum was 99.13%, indicating that the main metal contained in the leaching solution was aluminum, and the purity was very high.
[0056] The mass percentage content of nickel in the leaching residue (calculated based on the total mass of metals contained in the leaching residue) is 99.1%.
[0057] Example 4
[0058] This embodiment provides a method for treating nickel-aluminum waste to separate nickel and aluminum, and the raw materials treated are the same as those in Example 1.
[0059] The processing steps are as follows:
[0060] S1: placing a flux sodium hydroxide in a crucible, the molar number of the flux is 2.1 times the molar number of aluminum ions contained in the nickel-aluminum waste, heating and heating the sodium hydroxide in a microwave roasting furnace to melt the sodium hydroxide, the melting conditions are: microwave power 400W, roasting temperature 350°C, time control 7min; after the flux is melted, a spherical material (the ball diameter is controlled to be 1-2cm) prepared by mixing the nickel-aluminum waste and water is placed in a spoon, inserted from the top of the microwave roasting furnace, and suspended in the microwave roasting furnace for short-term activation, the short-term activation conditions are: microwave power 400W, roasting temperature 350°C, time control 2min;
[0061] S2: slowly pouring the short-time activated nickel-aluminum waste balls into the molten sodium hydroxide as a co-solvent, and roasting them in a microwave roasting furnace to obtain roasted slag; the microwave roasting conditions are controlled as follows: microwave power 500W, roasting temperature 550°C, and time controlled to 15min;
[0062] S3: The calcined slag (spherical) is first added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 5.0 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 90° C., stirred for 25 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0063] After testing and analysis, most of the aluminum in the raw nickel-aluminum waste entered the leaching solution, the aluminum recovery rate was 98%, and the nickel leaching rate was 0.07%. Calculated by the total mass of metals in the leaching solution (excluding sodium), the mass fraction of aluminum was 99.26%, indicating that the main metal contained in the leaching solution was aluminum, and the purity was very high.
[0064] The mass percentage content of nickel in the leached slag (calculated based on the total mass of metals contained in the leached slag) is 99.6%.
[0065] It can be seen from the above examples that the method of the present invention can be used to leach most of the aluminum in the nickel-aluminum waste, and the recovery rate of aluminum can reach up to 99%. At the same time, the leaching rate of nickel is low, below 0.1%, and the obtained leaching solution has high purity, which greatly simplifies the subsequent purification process of aluminum. The nickel content (calculated by the total weight of metal) in the leached residue after leaching is greater than 99%, and the purity is high. The leached residue can be directly used as a raw material for preparing a nickel-based catalyst after simple treatment.
[0066] Comparative Example 1
[0067] This comparative example provides a method for treating nickel-aluminum waste to separate nickel and aluminum, and the raw materials treated are the same as those in Example 1.
[0068] The processing steps are as follows:
[0069] S1: placing a flux sodium hydroxide in a crucible, the molar number of the flux is 2.1 times the molar number of aluminum ions contained in the nickel-aluminum waste, heating and heating the sodium hydroxide in a microwave roasting furnace to melt the sodium hydroxide, the melting conditions are: microwave power 400W, roasting temperature 350°C, time control 7min; after the flux is melted, placing the nickel-aluminum waste raw material (powder, not balled) in a spoon, inserting it from the top of the microwave roasting furnace, hanging it in the microwave roasting furnace for short-term activation, the short-term activation conditions are: microwave power 400W, roasting temperature 350°C, time control 2min;
[0070] S2: slowly pouring the short-time activated nickel-aluminum waste into the molten sodium hydroxide as a co-solvent, and roasting in a microwave roasting furnace to obtain roasted slag; the microwave roasting conditions are controlled as follows: microwave power 500W, roasting temperature 550°C, and time control 15min;
[0071] S3: The calcined slag is firstly added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 5.0 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 90° C., stirred for 25 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0072] After testing and analysis, the aluminum recovery rate of this comparative example is only 78%, the nickel content (calculated by the total weight of metal) in the leached residue after leaching is less than 20%, and the nickel and aluminum in the nickel-aluminum waste are not effectively separated.
[0073] It is believed that when powdered raw materials are directly added to the molten flux under the microwave field, it is easy to cause instantaneous agglomeration and wrapping problems, which will inevitably lead to a decrease in the recovery rate of aluminum. Previous studies have shown that pelletizing can avoid this phenomenon. At the same time, under the microwave field, the pellets can initially present a loose and porous structure, providing conditions and channels for the in-depth destruction of microwaves, forming a synergistic effect with the molten flux, and realizing the smooth progress of the subsequent leaching reaction.
[0074] Comparative Example 2
[0075] This comparative example provides a method for treating nickel-aluminum waste to separate nickel and aluminum, and the raw materials treated are the same as those in Example 1.
[0076] The processing steps are as follows:
[0077] S1: Potassium hydroxide, a flux, is placed in a crucible, the molar number of the flux is 2.0 times the molar number of aluminum ions contained in the nickel-aluminum waste, and the potassium hydroxide is melted by heating in a muffle furnace, and the melting conditions are: roasting temperature 400°C, and the time is controlled to be 6 minutes; after the flux is melted, a spherical material (the ball diameter is controlled to be 1-2 cm) prepared by mixing the nickel-aluminum waste and water is placed in a spoon, inserted from the top of the muffle furnace, and hung in the furnace for short-term activation, and the conditions for short-term activation are: roasting temperature 400°C, and the time is controlled to be 5 minutes;
[0078] S2: slowly pouring the short-time activated nickel-aluminum waste balls into the molten auxiliary solvent potassium hydroxide, and roasting them in a muffle furnace to obtain roasted slag; the roasting conditions are controlled as follows: the roasting temperature is 550°C and the time is controlled as 30 minutes;
[0079] S3: The calcined slag is firstly added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 4.0 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 80° C., stirred for 20 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0080] The calcination temperature in step S2 of this comparative example was changed from 550°C to 650°C, 750°C, 850°C, and 950°C, respectively, while the processing time remained unchanged. Experiments were carried out and the metal aluminum recovery rates at the corresponding temperatures were obtained. The results are shown in Table 2.
[0081] Table 2
[0082] Roasting temperature of slag, ℃ 550 650 750 850 950 Aluminum recovery rate, % 39 51 62 73 86
[0083] It can be seen from the above table that the NiAl content in the nickel-aluminum waste is 26 O 40 The phase is also difficult to decompose under low temperature conditions, indicating that it is difficult to destroy its chemical bonds under the roasting conditions. When the temperature is raised to 950 degrees, the aluminum recovery rate is also less than 90%, and the nickel content (calculated by the total weight of the metal) in the leached slag is less than 25%, and the nickel-aluminum separation effect is not ideal.
[0084] Experimental Example 1
[0085] This experimental example mainly investigates the effect of different short-term activation treatment times on aluminum recovery. The raw material nickel aluminum waste treated is the same as in Example 1.
[0086] The experimental steps are as follows:
[0087] S1: placing a flux sodium hydroxide in a crucible, the molar number of the flux is 1.8 times the molar number of aluminum ions contained in the nickel-aluminum waste, heating and heating the sodium hydroxide in a microwave roasting furnace to melt the sodium hydroxide, the melting conditions are: microwave power 400W, roasting temperature 350°C, time control 8min; after the flux is melted, a spherical material (the ball diameter is controlled to be 1-2cm) prepared by mixing the nickel-aluminum waste and water is placed in a spoon, inserted from the top of the microwave roasting furnace, and suspended in the microwave roasting furnace for short-time activation, the short-time activation conditions are: microwave power 400W, roasting temperature 350°C, and short-time activation time is controlled to be 0.5min;
[0088] S2: slowly pouring the short-time activated nickel-aluminum waste balls into the molten sodium hydroxide as a co-solvent, and roasting them in a microwave roasting furnace to obtain roasted slag; the microwave roasting conditions are controlled as follows: microwave power 1000W, roasting temperature 750°C, and time control 10min;
[0089] S3: The calcined slag (spherical) is first added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 2.5 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 70° C., stirred for 25 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0090] Only the short-time activation time in step S1 was set to 1 min, 2 min, 3 min, 3.5 min, and 4 min, respectively. The other steps and parameters were the same as the above steps, and experiments were carried out respectively.
[0091] After testing and analysis, the recovery rate of aluminum under different short-term activation times was obtained, and the experimental results are shown in Table 3 below.
[0092] Table 3
[0093] Short-term activation time, min 0.5 1 2 3 3.5 4 Aluminum recovery rate, % 76 98 99 98 90 84
[0094] It can be seen from the above experiments that activation treatment that is too short or too long is not conducive to the dissolution of aluminum in nickel-aluminum waste. If the time is too short, it is not conducive to promoting the formation of a loose and porous structure of the pellets. If the time is too long, due to the temperature difference between the raw materials and water, it is easy to increase the phenomenon of pellet powder falling off, which is not conducive to the subsequent contact reaction with the molten flux. Therefore, it is very important to control the short-term activation time. The preferred short-term activation time is 1 to 3 minutes.
[0095] Experimental Example 2
[0096] This experimental example mainly investigates the effect of different melting treatment times of flux on aluminum recovery rate. The raw material nickel aluminum waste treated is the same as that in Example 1.
[0097] The experimental steps are as follows:
[0098] S1: placing a flux sodium hydroxide in a crucible, the molar number of the flux is 1.8 times the molar number of aluminum ions contained in the nickel-aluminum waste, heating and heating the sodium hydroxide in a microwave roasting furnace to melt the sodium hydroxide, the melting conditions are: microwave power 400W, roasting temperature 350°C, time control 4min; after the flux is melted, placing a spherical material (the diameter of the ball is controlled to be 1-2cm) prepared by mixing the nickel-aluminum waste and water in a spoon, inserting it from the top of the microwave roasting furnace, and hanging it in the microwave roasting furnace for short-time activation, the conditions for short-time activation are: microwave power 400W, roasting temperature 350°C, and short-time activation time control 3min;
[0099] S2: slowly pouring the short-time activated nickel-aluminum waste balls into the molten sodium hydroxide as a co-solvent, and roasting them in a microwave roasting furnace to obtain roasted slag; the microwave roasting conditions are controlled as follows: microwave power 1000W, roasting temperature 750°C, and time control 10min;
[0100] S3: The calcined slag (spherical) is first added with water to prepare a hydrated calcined slag material, the liquid-to-solid ratio of the hydrated calcined slag material is 2.5 mL / g, the hydrated calcined slag material is subjected to water immersion treatment, the hydrated calcined slag material is heated to 70° C., stirred for 25 min, and then solid-liquid separated to obtain aluminum-containing leaching solution and nickel-containing leaching slag, respectively.
[0101] Only the melting time of sodium hydroxide in step S1 was set to 5 min, 6 min, 7 min, 8 min, 9 min, and 10 min, respectively, and the other steps and parameters were the same as the above steps, and experiments were carried out respectively.
[0102] After testing and analysis, the recovery rate of aluminum under different melting times was obtained, and the experimental results are shown in Table 4 below.
[0103] Table 4
[0104] Flux melting time, min 4 5 6 7 8 9 10 Aluminum recovery rate, % 83 98 98 99 98 89 86
[0105] Through the above experiments, it can be seen that too short or too long melting time of the flux is not conducive to the dissolution of aluminum in nickel-aluminum waste. If the time is too short, the melting is incomplete. If the time is too long, it is easy to cause overheating inside the flux, causing the internal chemical structure of the flux to change, which is not conducive to the subsequent contact roasting reaction with the nickel-aluminum waste balls and it is difficult to form a synergistic effect. Therefore, it is also very important to control the melting time of the flux. The preferred melting time of the flux is 5 to 8 minutes.
[0106] The above examples illustrate that the method of the present invention can achieve the recovery of insoluble NiAl in difficult-to-treat nickel-aluminum waste. 26 O 40 The rapid and effective separation of aluminum and nickel in the physical phases results in a high purity leaching solution, which greatly simplifies the subsequent purification process of aluminum. The nickel purity in the leaching residue after leaching is high, and the leaching residue can be directly used as a raw material for the preparation of nickel-based catalysts after simple treatment.
[0107] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for treating nickel-aluminum waste to separate nickel-aluminum, characterized in that: Includes steps: S1: Mixing nickel-aluminum waste with water to make balls, the ball diameter is controlled to be 1-2 cm, and then short-term activation is performed in a microwave environment to obtain activated nickel-aluminum waste balls; wherein the conditions for short-time activation are: microwave power 300-500W, roasting temperature 350-450°C, and short-time activation time is controlled to be 1-3 min; wherein the nickel-aluminum waste is solid waste residue after waste nickel-aluminum powder is treated with strong alkali, and the nickel-aluminum waste contains insoluble NiAl 26 O 40 phase of matter; S2: Mixing the activated nickel-aluminum waste balls with melted flux, and roasting in a microwave environment to obtain roasted slag; the roasting conditions are: microwave power 500-1000W, roasting temperature 550-750°C; wherein the flux is melted in a microwave environment, and the melting conditions are: microwave power 300-500W, temperature 350-450°C, and time controlled to be 5-8 min; S3: treating the roasted slag by water leaching, and then performing solid-liquid separation to obtain an aluminum-containing leaching solution and a nickel-containing leaching slag.
2. The method according to claim 1, characterized in that The flux is sodium hydroxide and / or potassium hydroxide.
3. The method according to claim 2, characterized in that The molar number of the flux is 1.2 to 2.5 times the molar number of aluminum ions contained in the nickel-aluminum waste.
4. The method according to claim 1, characterized in that In step S2, when calcining in a microwave environment, the calcining time is controlled to be 10 to 15 minutes.
5. The method according to claim 4, characterized in that In step S3, the water immersion treatment conditions are: immersion temperature 70-90° C., and treatment time 20-30 min.
6. The method according to claim 5, characterized in that Before the calcined slag is treated by the water immersion method, water is first added to prepare a water-containing calcined slag material, and the liquid-to-solid ratio of the water-containing calcined slag material is 2.5-5.0 mL / g.
Citation Information
Patent Citations
Method for extracting nickel, aluminum and molybdenum by waste hydrogenation catalyst through microwave treatment
CN108504863A