Antibacterial fluororubber composite material and preparation method thereof
By using fluororubber composite materials in wearable devices, combined with components such as maleic anhydride acylated chitosan and silver-copper-zinc-doped titanium dioxide, the problem of insufficient antibacterial and heat dissipation properties of fluororubber materials is solved, achieving excellent Mechanical, thermal conductivity and antibacterial properties, suitable for wearable device applications.
Patent Information
- Application Number
- CN202410286357.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-13
AI Technical Summary
The fluororubber material in existing wearable devices has poor antibacterial effect and insufficient heat dissipation performance, especially when it comes into direct contact with the user's skin and requires frequent cleaning.
An antibacterial fluororubber composite material is used, including fluororubber, epoxy resin, plasticizer, coupling agent, thermally conductive filler, zinc oxide, zinc stearate, antioxidant, accelerator and composite antibacterial agent. The composite antibacterial agent is composed of It is composed of maleic anhydride acylated chitosan and silver-copper-zinc-doped titanium dioxide. The synergistic effect of these components improves the antibacterial performance and thermal conductivity of the material.
It achieves excellent mechanical properties, thermal conductivity, antibacterial properties and hydrophilicity, has a simple preparation process and fast vulcanization speed, and is suitable for the needs of the wearable device field.
Smart Images

Figure BDA0004739267620000091 
Figure BDA0004739267620000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of fluororubber materials, and in particular to an antibacterial fluororubber composite material and a preparation method thereof. Background Art
[0002] Rubber refers to a highly elastic polymer material with reversible deformation. It is elastic at room temperature, can produce large deformation under very small external force, and can return to its original shape after the external force is removed. Fluororubber refers to a synthetic polymer elastomer containing fluorine atoms on the carbon atoms of the main chain or side chain. The introduction of fluorine atoms can give rubber excellent heat resistance, oil resistance, oxidation resistance, corrosion resistance and atmospheric aging resistance. Due to the characteristics of high temperature resistance, high vacuum resistance, oil resistance, acid and alkali resistance, and resistance to a variety of chemicals, fluororubber has been used in modern aviation, rockets, missiles, space navigation, atomic energy, ships and other cutting-edge technologies and automotive, petroleum, shipbuilding, chemistry, machinery, telecommunications, instruments and other industrial fields. Wearable devices are portable devices that are worn directly on the body or integrated into the user's clothes or accessories. Since wearable devices need to focus on the wearing comfort and stability of the device and the user, fluororubber is also commonly used in wearable devices.
[0003] However, the fluororubber materials used in existing wearable devices have poor antibacterial effects and poor heat dissipation performance, and often need to be cleaned repeatedly after use, especially for fluororubber used in direct contact with the user's skin.
[0004] Therefore, a fluororubber composite material with good thermal conductivity, good antibacterial effect and durability is developed to meet market demand. Summary of the invention
[0005] The purpose of this application is to provide an antibacterial fluororubber composite material and a preparation method thereof in view of the deficiencies of the current technology.
[0006] In a first aspect, the present application provides an antibacterial fluororubber composite material, which adopts the following technical solution:
[0007] An antibacterial fluororubber composite material comprises the following raw materials by weight: 70-75 parts of fluororubber, 5-7 parts of epoxy resin E-51, 5-7 parts of plasticizer, 3-5 parts of coupling agent, 30-35 parts of thermal conductive filler, 5-8 parts of zinc oxide, 2-4 parts of zinc stearate, 1-1.5 parts of antioxidant, 1-1.5 parts of accelerator, 1-2 parts of vulcanizer and 2-3 parts of composite antibacterial agent, wherein the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a weight ratio of 5-7:1.
[0008] By adopting the above technical scheme, fluororubber: as a matrix resin, it provides the flexibility and wear resistance of the material. Epoxy resin E-51: plays a toughening role, improving the strength and durability of the material. Plasticizer: increases the softness and processability of the material. Coupling agent: improves the adhesion between the filler and the matrix resin, enhances the interface interaction, and improves the performance of the composite material. Thermal conductive filler: improves the thermal conductivity of the material, optimizes the thermal conductivity path, and improves the heat dissipation efficiency. Anti-aging agent: prevents material aging and extends the service life. Accelerator: accelerates the vulcanization reaction and increases the vulcanization speed. Vulcanizing agent: as a cross-linking agent, promotes the vulcanization of the material and enhances the wear resistance and anti-aging ability of the material. Composite antibacterial agent: composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide, it has excellent antibacterial efficiency and long-term antibacterial ability. The synergistic effect of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide can improve the antibacterial performance. Maleic anhydride acylated chitosan improves the antibacterial effect by increasing the hydrophilicity of the material. Silver, copper, zinc and other ions play an antibacterial role by killing bacteria and inhibiting their growth. The addition of composite antibacterial agents to the material can ensure that the antibacterial effect is long-lasting and stable. In short, the role and synergy of the various components in the antibacterial fluororubber composite material make the material have excellent mechanical properties, good thermal conductivity, excellent antibacterial properties and hydrophilicity, and the preparation process is simple, the vulcanization speed is fast, and it is energy-saving and environmentally friendly, which can meet the market demand for fluororubber composite materials in the field of wearable devices.
[0009] Preferably, the method for preparing silver-copper-zinc doped titanium dioxide comprises the following steps:
[0010] S21. At room temperature, add 200 mL of tetra-n-butyl titanate to 350 g of ethanol and stir for 20 min to form solution A.
[0011] S22, adding 1 g of silver nitrate, 5 g of copper nitrate and 8 g of zinc nitrate to a solution consisting of 70 g of ethanol, 20 mL of acetic acid and 50 mL of water to form solution B;
[0012] S23, adding solution B dropwise into solution A at a stirring speed of 200 rpm for 20 min, heating to 43°C, standing for aging for 10 h, then centrifuging, washing, drying at 90°C for 12 h, and finally calcining at 530°C for 2.5 h, cooling, and grinding to obtain silver-copper-zinc-doped titanium dioxide, wherein the particle size of the silver-copper-zinc-doped titanium dioxide is 0.1-0.2 microns.
[0013] By adopting the above technical scheme, the prepared silver, copper and zinc doped titanium dioxide plays the role of a composite antibacterial agent, and has excellent antibacterial efficiency and long-term antibacterial ability. The synergistic effect of maleic anhydride acylated chitosan and silver, copper and zinc doped titanium dioxide can improve the hydrophilicity and antibacterial properties of the material. Maleic anhydride acylated chitosan increases the hydrophilicity of the material, making it have better water solubility and hydrophilicity, thereby improving the antibacterial effect. In addition, silver, copper and zinc doped titanium dioxide has a smaller particle size range (0.1-0.2 microns), which can provide a larger specific surface area, increase the release of active ions such as silver, copper and zinc, and thus enhance the antibacterial properties. In summary, the preparation method of silver, copper and zinc doped titanium dioxide and the effect and synergistic effect of adding it to antibacterial fluororubber composite materials can provide excellent antibacterial effects and long-term antibacterial ability, and meet the market demand for fluororubber composite materials in the field of wearable devices by improving the hydrophilicity and antibacterial properties of the material.
[0014] Preferably, the preparation method of maleic anhydride acylated chitosan is as follows: 12g chitosan is uniformly dispersed in 1000mL deionized water under stirring, then 4g sodium carbonate is added, and after stirring for 30min, 40g maleic anhydride is added, and after mixing for 8h, stirring is stopped, potassium hydroxide is added, the pH value is adjusted to 10, and the unreacted chitosan and the solution are separated by high-speed centrifugation, hydrochloric acid is added to the solution, the pH value is adjusted to a large amount of floccules are precipitated, centrifugation is performed, the precipitate is washed with acetone, vacuum dried, and allowed to stand for 24h to obtain maleic anhydride acylated chitosan.
[0015] By adopting the above technical scheme, maleic anhydride acylated chitosan is an important component in the antibacterial fluororubber composite material, which is prepared by the following steps: chitosan is uniformly dispersed in deionized water under stirring, sodium carbonate and maleic anhydride are added for reaction, and then centrifuged and washed to obtain. After the maleic anhydride acylated chitosan is added to the composite material, its hydrophilicity can be increased, so that the material has better water wettability, thereby improving the antibacterial ability and antifouling performance of the material. Maleic anhydride acylated chitosan has a special chemical structure and can react with antibacterial agents such as silver, copper and zinc doped titanium dioxide to form a composite antibacterial agent. This composite antibacterial agent can release active ions (such as silver ions, copper ions and zinc ions), and has excellent antibacterial effect and long-term antibacterial ability. Therefore, maleic anhydride acylated chitosan can improve the hydrophilicity and antibacterial properties of the material in the antibacterial fluororubber composite material, and play a synergistic role. It cooperates with other components such as silver, copper and zinc doped titanium dioxide in the material, which can provide better antibacterial effect and meet the market demand for fluororubber composite materials in the field of wearable devices.
[0016] Preferably, the method for preparing the thermally conductive filler comprises the following steps:
[0017] S41, according to the weight ratio, 1.6 parts of vinyltrimethoxysilane, 200 parts of isopropanol and 200 parts of water were mixed and stirred to obtain a mixture C;
[0018] S42, adding 100 parts of aluminum nitride and 50 parts of boron nitride to mixture C according to their mass fractions; then heating to 45° C. and stirring at a speed of 200 r / min for 120 min to obtain a silanized thermal conductive filler mixed liquid;
[0019] S43. The silanized thermal conductive filler mixture is filtered, washed with ethanol, dried at 75°C, ground, and then subjected to plasma surface modification for 15 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a thermal flame retardant filler with an average particle size of 5-10 μm.
[0020] By adopting the above technical scheme, in the antibacterial fluororubber composite material of the present application, the raw materials for preparing the thermal conductive filler and the composite antibacterial agent are modified by different methods respectively, and play different roles, but the two have a synergistic effect in the material. The thermal conductive filler is obtained by vinyl trimethoxysilane modification and plasma surface modification, and its main functions are: the thermal conductive filler is uniformly dispersed in the fluororubber matrix resin, and forms a continuous three-dimensional thermal conductive filler network, which can greatly improve the thermal conductivity of the composite material, thereby improving the heat dissipation effect of the material. Through vinyl trimethoxysilane modification and plasma surface modification, the compatibility and dispersibility of the thermal conductive filler with components such as fluororubber and epoxy resin are improved, so that the components of the composite material are more evenly mixed, and the overall performance of the material is improved. The thermal conductive filler has a synergistic effect with the composite antibacterial agent in the material, which is mainly reflected in: the continuous three-dimensional network of the thermal conductive filler can promote the uniform dispersion of the composite antibacterial agent in the material, and provide a larger contact area, thereby improving the antibacterial efficiency of the composite antibacterial agent. The addition of the composite antibacterial agent can increase the antibacterial property of the surface of the thermal conductive filler, and effectively improve the antibacterial property of the material.
[0021] Preferably, the plasticizer is one of ethylene-octene copolymer and ethylene-vinyl acetate copolymer, the mass content of octene in the ethylene-octene copolymer is 25-30%; the mass content of vinyl acetate in the ethylene-vinyl acetate copolymer is 10-20%.
[0022] Preferably, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 2-4:3:1.
[0023] By adopting the above technical scheme, in the present application, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N, N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 2-4:3:1. The coupling agent has the following effects and synergistic effects in the antibacterial fluororubber composite material: the coupling agent has silicon-friendly and glue-friendly properties, and can effectively combine with components such as fluororubber matrix resin and epoxy resin E-51, improve the compatibility between them, and enhance the dispersibility of thermally conductive fillers in the composite material. The addition of coupling agents can form chemical bonds or physical bonds, enhance the bonding force between thermally conductive fillers and components such as fluororubber matrix resin and epoxy resin E-51, and improve the mechanical properties and comprehensive properties of the composite material. The addition of coupling agents can improve the dispersion and filling effect of thermally conductive fillers in the material, further enhance the thermal conductivity of thermally conductive fillers, and improve the thermal conductivity of composite materials. The coupling agent interacts with other components such as the composite antimicrobial agent and thermal conductive filler, which can promote a more uniform dispersion of the composite antimicrobial agent and provide a better thermal conductivity path, thereby improving the thermal conductivity and antimicrobial properties of the material. In summary, the role of the coupling agent in antimicrobial fluororubber composite materials is mainly to promote compatibility and dispersibility, enhance interfacial adhesion and improve thermal conductivity, and work synergistically with other components to jointly improve the performance of the material.
[0024] Preferably, the vulcanizing agent is bisphenol AF.
[0025] Preferably, the antioxidant is at least one of antioxidant MB and antioxidant MC.
[0026] Preferably, the accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:3.
[0027] In a second aspect, the present application provides a method for preparing an antibacterial fluororubber composite material, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned antibacterial fluororubber composite material, comprising the following steps:
[0028] S101, according to the mass fraction, fluororubber, epoxy resin E-51 and plasticizer are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between two rollers for plasticization for 30-35min, and then coupling agent, zinc oxide, zinc stearate, antioxidant, accelerator and composite antibacterial agent are added step by step in sequence for mixing for 5-8min, and after being evenly dispersed, thermal conductive filler is added, and after the addition is completed, cutting and refining are performed 4 times, and finally a vulcanizing agent is added, and after mixing is evenly, thinning is passed 6-8 times, and the rubber is pounded and sliced to obtain a mixed rubber, which is aged for standby use;
[0029] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 190-210°C, pre-compression pressure 8-10MPa, vulcanization pressure 15-17MPa, vulcanization time 8-12min, to obtain an antibacterial fluororubber composite material.
[0030] In summary, the beneficial technical effects of this application are:
[0031] 1. Excellent mechanical properties: Fluororubber composite materials have excellent mechanical properties such as wear resistance, tear resistance and tensile strength, and are suitable for applications in various wearable devices.
[0032] 2. Excellent thermal conductivity: The thermal conductive filler is evenly dispersed in the fluororubber matrix resin to form a continuous three-dimensional thermal conductive filler network, which effectively improves the thermal conductivity of the composite material and is suitable for application scenarios that require better heat dissipation performance.
[0033] 3. Excellent antibacterial properties: The composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver, copper and zinc doped titanium dioxide. It has excellent antibacterial effect and long-term antibacterial properties, can prevent the growth and reproduction of bacteria, and has high hygiene properties.
[0034] 4. Good hydrophilicity: Adding maleic anhydride acylated chitosan can improve the hydrophilicity of the composite material, making it have excellent wettability and lubricity, and enhancing the ease of use of the material.
[0035] 5. The preparation process is simple and the vulcanization speed is fast: The process of preparing the composite material is relatively simple and the vulcanization speed is fast, which improves production efficiency, saves energy and reduces environmental pollution. DETAILED DESCRIPTION
[0036] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0037] Preparation Example 1 Preparation of copper-zinc-doped titanium dioxide
[0038] The preparation method of silver-copper-zinc doped titanium dioxide comprises the following steps:
[0039] S21. At room temperature, add 200 mL of tetra-n-butyl titanate to 350 g of ethanol and stir for 20 min to form solution A.
[0040] S22, adding 1 g of silver nitrate, 5 g of copper nitrate and 8 g of zinc nitrate to a solution consisting of 70 g of ethanol, 20 mL of acetic acid and 50 mL of water to form solution B;
[0041] S23, adding solution B dropwise into solution A at a stirring speed of 200 rpm for 20 min, heating to 43°C, standing for aging for 10 h, then centrifuging, washing, drying at 90°C for 12 h, and finally calcining at 530°C for 2.5 h, cooling, and grinding to obtain silver-copper-zinc-doped titanium dioxide, wherein the particle size of the silver-copper-zinc-doped titanium dioxide is 0.1-0.2 microns.
[0042] Preparation Example 2 Preparation of maleic anhydride acylated chitosan
[0043] The preparation method of maleic anhydride acylated chitosan is as follows: 12g chitosan is uniformly dispersed in 1000mL deionized water under stirring, and then 4g sodium carbonate is added, and after stirring and reacting for 30min, 40g maleic anhydride is added, and after mixing and reacting for 8h, stirring is stopped, potassium hydroxide is added, the pH value is adjusted to 10, and the unreacted chitosan and the solution are separated by high-speed centrifugation, hydrochloric acid is added to the solution, the pH value is adjusted to a large amount of flocs precipitate, centrifugation is performed, the precipitate is washed with acetone, vacuum dried, and allowed to stand for 24h to obtain maleic anhydride acylated chitosan.
[0044] Preparation Example 3
[0045] The preparation method of the thermal conductive filler comprises the following steps:
[0046] S41, according to the mass fractions, 1.6 g of vinyltrimethoxysilane, 200 g of isopropanol and 200 g of water were mixed and stirred to obtain a mixture C;
[0047] S42, adding 100 g of aluminum nitride and 50 g of boron nitride to mixture C according to their mass fractions; then heating to 45° C. and stirring at a speed of 200 r / min for 120 min to obtain a silanized thermal conductive filler mixed liquid;
[0048] S43. The silanized thermal conductive filler mixture is filtered, washed with ethanol, dried at 75°C, ground, and then subjected to plasma surface modification for 15 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a thermal flame retardant filler with an average particle size of 5-10 μm.
[0049] Preparation Comparative Example 1
[0050] Same as Preparation Example 3, except that the reaction was not modified by plasma.
[0051] Example 1
[0052] An antibacterial fluororubber composite material comprises the following raw materials by weight: 7kg of fluororubber, 0.5kg of epoxy resin E-51, 0.5kg of ethylene-octene copolymer (the mass content of octene in the ethylene-octene copolymer is 25%), 0.3kg of coupling agent, 3kg of thermal conductive filler, 0.5kg of zinc oxide, 0.2kg of zinc stearate, 0.1kg of antioxidant MB, 0.1kg of accelerator, 0.1kg of bisphenol AF, and 0.2kg of composite antibacterial agent, wherein the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a mass ratio of 5:1, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 2:3:1; and the accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:3.
[0053] The method for preparing the above-mentioned antibacterial fluororubber composite material comprises the following steps:
[0054] S101, according to the mass fractions, fluororubber, epoxy resin E-51 and ethylene-octene copolymer (the mass content of octene in the ethylene-octene copolymer is 25%) are mixed uniformly, the roller distance of the open mill is adjusted, the mixture is placed between two rollers for plastication for 30 minutes, and then coupling agent, zinc oxide, zinc stearate, antioxidant MB, accelerator and composite antibacterial agent are added step by step in sequence for mixing for 5 minutes, after being evenly dispersed, thermal conductive filler is added, and after the addition is completed, cutting and refining are performed for 4 times, and finally bisphenol AF is added, and after mixing is evenly, thinning is performed for 6 times, and the rubber is pounded and sliced to obtain a mixed rubber, which is aged for standby use;
[0055] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 190° C., pre-compression pressure 8 MPa, vulcanization pressure 15 MPa, vulcanization time 8 min, to obtain an antibacterial fluororubber composite material.
[0056] Example 2
[0057] An antibacterial fluororubber composite material comprises the following raw materials by weight: 7.5 kg of fluororubber, 0.7 kg of epoxy resin E-51, 0.7 kg of ethylene-vinyl acetate copolymer (the mass content of vinyl acetate in the ethylene-vinyl acetate copolymer is 10%), 0.5 kg of coupling agent, 3.5 kg of thermal conductive filler, 0.8 kg of zinc oxide, 0.4 kg of zinc stearate, 0.15 kg of antioxidant MC, 0.15 kg of accelerator, 0.2 kg of bisphenol AF, and 0.3 kg of composite antibacterial agent, wherein the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a mass ratio of 7:1, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 4:3:1; and the accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:3.
[0058] The method for preparing the above-mentioned antibacterial fluororubber composite material comprises the following steps:
[0059] S101, according to the mass fractions, fluororubber, epoxy resin E-51 and ethylene-vinyl acetate copolymer (the mass content of vinyl acetate in ethylene-vinyl acetate copolymer is 10%) are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between two rollers for plastication for 35 minutes, and then coupling agent, zinc oxide, zinc stearate, antioxidant MC, accelerator and composite antibacterial agent are added step by step in sequence for mixing for 8 minutes, and after being evenly dispersed, heat conductive filler is added, and after the addition is completed, cutting and refining are performed for 4 times, and finally bisphenol AF is added, and after mixing is evenly, thinning is performed for 8 times, and the rubber is pounded and sliced to obtain a mixed rubber, which is aged for standby use;
[0060] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 210° C., pre-compression pressure 10 MPa, vulcanization pressure 17 MPa, vulcanization time 12 min, to obtain an antibacterial fluororubber composite material.
[0061] Example 3
[0062] An antibacterial fluororubber composite material comprises the following raw materials by weight: 7.3 kg of fluororubber, 0.6 kg of epoxy resin E-51, 0.6 kg of ethylene-octene copolymer (the mass content of octene in the ethylene-octene copolymer is 30%), 0.4 kg of coupling agent, 3.3 kg of thermal conductive filler, 0.7 kg of zinc oxide, 0.3 kg of zinc stearate, 0.12 kg of antioxidant MB, 0.13 kg of accelerator, 0.15 kg of bisphenol AF, and 0.25 kg of composite antibacterial agent, wherein the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a mass ratio of 6:1, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 3:3:1; and the accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:3.
[0063] The method for preparing the above-mentioned antibacterial fluororubber composite material comprises the following steps:
[0064] S101, according to the mass fractions, fluororubber, epoxy resin E-51 and ethylene-octene copolymer (the mass content of octene in the ethylene-octene copolymer is 30%) are mixed uniformly, the roller distance of the open mill is adjusted, the mixture is placed between two rollers for plastication for 33 minutes, and then coupling agent, zinc oxide, zinc stearate, antioxidant MB, accelerator and composite antibacterial agent are added step by step in sequence for mixing for 7 minutes, after being evenly dispersed, heat conductive filler is added, and after the addition is completed, cutting and refining are performed for 4 times, and finally bisphenol AF is added, and after mixing is evenly, thinning is performed for 7 times, and the rubber is pounded and sliced to obtain a mixed rubber, which is aged for standby use;
[0065] S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 200° C., pre-compression pressure 9 MPa, vulcanization pressure 16 MPa, vulcanization time 10 min, to obtain an antibacterial fluororubber composite material.
[0066] Example 4
[0067] The same as Example 3, except that an equal amount of γ-aminopropyltriethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 3:3:1.
[0068] Example 5
[0069] The same as Example 3, except that an equal amount of vinyltrimethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 3:3:1.
[0070] Example 6
[0071] The same as Example 3, except that an equal amount of N,N-diethylaminopropylmethyldimethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 3:3:1.
[0072] Example 7
[0073] The same as Example 3, except that an equal amount of accelerator CZ is used to replace the accelerator, and the accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:3.
[0074] Example 8
[0075] The same as Example 3, except that an equal amount of accelerator TMTD is used to replace the accelerator, and the accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:3.
[0076] Comparative Example 1
[0077] The same as Example 3, except that an equal amount of the thermally conductive filler prepared in Preparation Comparative Example 1 is used instead of the thermally conductive filler prepared in Preparation Example 3.
[0078] Comparative Example 2
[0079] The same as Example 3, except that an equal amount of aluminum nitride (the average particle size of aluminum nitride is 5-10 μm) is used to replace the thermal conductive filler prepared in Preparation Example 3.
[0080] Comparative Example 3
[0081] The same as Example 3, except that an equal amount of boron nitride (the average particle size of the boron nitride is 5-10 μm) is used to replace the thermally conductive filler prepared in Preparation Example 3.
[0082] Comparative Example 4
[0083] The same as Example 3, except that an equal amount of maleic anhydride acylated chitosan is used to replace the composite antibacterial agent, and the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a mass ratio of 6:1.
[0084] Comparative Example 5
[0085] The same as Example 3, except that an equal amount of silver-copper-zinc doped titanium dioxide is used instead of the composite antibacterial agent, and the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a mass ratio of 6:1.
[0086] Performance Testing
[0087] The antibacterial fluororubber composite materials prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were sampled and tested. The test results are shown in Table 1.
[0088] Thermal conductivity: Refer to "GB / T32064-2015 Transient Plane Heat Source Test Method for Thermal Conductivity and Thermal Diffusivity of Building Materials", and use TPS2500S thermal constant analyzer for testing;
[0089] Shore A hardness is tested according to GB / T 531.1-2008;
[0090] The tensile properties were tested according to GB / T528-2009. The test length and width of the dumbbell-shaped specimen were 75 mm and 4 mm respectively, and the tensile rate was 500 mm min. -1 ;
[0091] Hydrophilicity: tested with a contact angle meter, the solvent is water;
[0092] Antibacterial performance: tested in accordance with GB / T31402-2015;
[0093] Tear strength: According to GB / T 6039-85, tear strength is defined as the maximum force applied to the specimen in a direction parallel to the main axis of the specimen until it cracks. The specimens are prepared according to the methods of GB529 and GB530. The test steps are as follows: (1) The vulcanized test piece (thickness 2.0±0.3mm) should be left at standard room temperature (not less than 6 hours and not more than 15 days); (2) When taking the specimen, the direction of the bisector of the tear angle of the cutter should be consistent with the calendering direction; (3) The specimen is clamped vertically in the upper and lower clamps to a certain depth and clamped evenly at equal positions; (4) The tensile speed is adjusted (running at a speed of 500±100mm / min in the clamp) and the testing machine is started. A gradually increasing traction force can be applied to the specimen until the specimen is torn and then the machine is stopped.
[0094] Table 1 Performance test
[0095]
[0096]
[0097] Analyzing the data in Table 1, we can see that:
[0098] 1) The antibacterial fluororubber composite materials prepared in Examples 1 to 3 have excellent mechanical properties, good thermal conductivity, superior antibacterial properties and good hydrophilicity, simple preparation process, fast vulcanization speed, energy saving and environmental protection, and are very suitable for the market demand in the field of wearable devices.
[0099] 2) By comparing the performance of the antibacterial fluororubber composite materials prepared in Example 3 and Example 4-Example 6, a coupling agent consisting of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 3:3:1 is used, and the synergistic effect therebetween is utilized to improve the comprehensive performance of the antibacterial fluororubber composite material.
[0100] 3) A comparative analysis of the performance of the antibacterial fluororubber composite material was obtained by combining Example 3 with Example 7-Example 8. An accelerator consisting of accelerator CZ and accelerator TMTD in a mass ratio of 2:3 was used. The synergistic effect between them was utilized to increase the vulcanization reaction rate and the cross-linking effect, and to promote the rubber molecules in the composite material to better interact with other components, thereby enhancing the performance of the composite material.
[0101] 4) Based on the comparative analysis of the performance of the antibacterial fluororubber composite materials obtained in Example 3 and Comparative Example 1, the thermal conductive filler is modified by oxygen plasma to improve the interface compatibility, thereby improving the comprehensive performance of the antibacterial fluororubber composite material.
[0102] 5) In combination with the comparative analysis of the performance of the antibacterial fluororubber composite materials prepared in Example 3 and Comparative Examples 2-3, the thermal conductive filler prepared in Preparation Example 3 is used, and after the synergistic effect between aluminum nitride and boron nitride and vinyl trimethoxysilane modification, it is subjected to plasma modification treatment to form a continuous three-dimensional thermal conductive filler network in the rubber matrix resin, which significantly improves the thermal conductivity of the antibacterial fluororubber composite material. Through vinyl trimethoxysilane modification and plasma modification, its compatibility and dispersibility with the rubber matrix are improved, and the comprehensive performance of the antibacterial fluororubber composite material is further improved.
[0103] 6) In combination with the comparative analysis of the performance of the antibacterial fluororubber composite materials prepared in Example 3 and Comparative Examples 4-5, a composite antibacterial agent consisting of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a mass ratio of 6:1 was used, and the synergistic effect between them was utilized to further improve the antibacterial properties of the antibacterial fluororubber composite material.
[0104] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. An antibacterial fluororubber composite material, characterized in that: The preparation material comprises the following raw materials by weight: 70-75 parts of fluororubber, 5-7 parts of epoxy resin E-51, 5-7 parts of plasticizer, 3-5 parts of coupling agent, 30-35 parts of thermal conductive filler, 5-8 parts of zinc oxide, 2-4 parts of zinc stearate, 1-1.5 parts of antioxidant, 1-1.5 parts of accelerator, 1-2 parts of vulcanizing agent, and 2-3 parts of composite antibacterial agent, wherein the composite antibacterial agent is composed of maleic anhydride acylated chitosan and silver-copper-zinc doped titanium dioxide in a weight ratio of 5-7:1; The preparation method of silver-copper-zinc doped titanium dioxide comprises the following steps: S21. At room temperature, add 200 mL of tetra-n-butyl titanate to 350 g of ethanol and stir for 20 min to form solution A. S22, adding 1 g of silver nitrate, 5 g of copper nitrate and 8 g of zinc nitrate to a solution consisting of 70 g of ethanol, 20 mL of acetic acid and 50 mL of water to form solution B; S23, adding solution B dropwise into solution A at a stirring speed of 200 rpm for 20 min, heating to 43° C., standing for 10 h, then centrifuging, washing, drying at 90° C. for 12 h, and finally calcining at 530° C. for 2.5 h, cooling, and grinding to obtain silver-copper-zinc-doped titanium dioxide, wherein the particle size of the silver-copper-zinc-doped titanium dioxide is 0.1-0.2 μm; The preparation method of maleic anhydride acylated chitosan is as follows: 12g chitosan is uniformly dispersed in 1000mL deionized water under stirring, then 4g sodium carbonate is added, and after stirring for 30min, 40g maleic anhydride is added, and after mixing for 8h, stirring is stopped, potassium hydroxide is added, the pH value is adjusted to 10, and the unreacted chitosan and the solution are separated by high-speed centrifugation, hydrochloric acid is added to the solution, the pH value is adjusted until a large amount of floccules are precipitated, centrifugation is performed, the precipitate is washed with acetone, vacuum dried, and allowed to stand for 24h to obtain maleic anhydride acylated chitosan; The preparation method of the thermal conductive filler comprises the following steps: S41, according to the weight ratio, 1.6 parts of vinyltrimethoxysilane, 200 parts of isopropanol and 200 parts of water were mixed and stirred to obtain a mixture C; S42, adding 100 parts of aluminum nitride and 50 parts of boron nitride to mixture C according to their mass fractions; then heating to 45° C. and stirring at a speed of 200 r / min for 120 min to obtain a silanized thermal conductive filler mixed liquid; S43. The silanized thermal conductive filler mixture is filtered, washed with ethanol, dried at 75°C, ground, and then subjected to plasma surface modification for 15 seconds at a power of 2 kW and an oxygen volume concentration of 10% to obtain a thermal flame retardant filler with an average particle size of 5-10 μm.
2. The antibacterial fluororubber composite material according to claim 1, characterized in that: The plasticizer is one of ethylene-octene copolymer and ethylene-vinyl acetate copolymer, the mass content of octene in the ethylene-octene copolymer is 25-30%; the mass content of vinyl acetate in the ethylene-vinyl acetate copolymer is 10-20%.
3. The antibacterial fluororubber composite material according to claim 1, characterized in that: The coupling agent is composed of gamma-aminopropyltriethoxysilane, vinyltrimethoxysilane and N,N-diethylaminopropylmethyldimethoxysilane in a mass ratio of 2-4:3:
1.
4. The antibacterial fluororubber composite material according to claim 1, characterized in that: The vulcanizing agent is bisphenol AF.
5. The antibacterial fluororubber composite material according to claim 1, characterized in that: The antioxidant is at least one of antioxidant MB and antioxidant MC.
6. The antibacterial fluororubber composite material according to claim 1, characterized in that: The accelerator is composed of accelerator CZ and accelerator TMTD in a mass ratio of 2:
3.
7. A method for preparing an antibacterial fluororubber composite material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S101, according to the mass fraction, fluororubber, epoxy resin E-51 and plasticizer are mixed uniformly, the roller distance of the open mill is adjusted, and the mixture is placed between two rollers for plasticization for 30-35min, and then coupling agent, zinc oxide, zinc stearate, antioxidant, accelerator and composite antibacterial agent are added step by step in sequence for mixing for 5-8min, and after being evenly dispersed, thermal conductive filler is added, and after the addition is completed, cutting and refining are performed 4 times, and finally a vulcanizing agent is added, and after mixing is evenly, thinning is passed 6-8 times, and the rubber is pounded and sliced to obtain a mixed rubber, which is aged for standby use; S102, placing the aged rubber mixture in a flat vulcanizer for vulcanization, the vulcanization process is: temperature 190-210°C, pre-compression pressure 8-10MPa, vulcanization pressure 15-17MPa, vulcanization time 8-12min, to obtain an antibacterial fluororubber composite material.
Citation Information
Patent Citations
Antibacterial aging-resistant modified fluororubber composite material
CN105367956A
Antibacterial synthetic resin and preparation method thereof
CN108164951A
Application of reduced metal oxide semiconductor nanomaterial in antibacterial material
CN113827720A
Fluororubber composite material for antibacterial wearable equipment and preparation method of fluororubber composite material
CN117186572A
Antibacterial modified plastic
WO2022022544A1