Method for preparing ceramic black pigment from waste steel slag
By performing multi-step treatment of scrap steel slag and forming nano-scale spinel, the problems of low blackness and unstable coloring of black ceramic colorants in the prior art are solved, and the effects of high purity and stable coloring are achieved.
Patent Information
- Application Number
- CN202410321478.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-03-20
AI Technical Summary
The existing methods of using scrap steel slag to prepare black ceramic colorants lead to low blackness and unstable coloring, color difference and poor quality.
The temperature control reaction was carried out by soaking, filtration, adjusting the pH by scrap steel slag, adding sodium sulfide and sodium chromate, and using sodium bentonite load to form nano-scale spinel, combined with ultrasonic oscillation and vacuum drying, and finally calcined and grinded to produce a high-purity black color. material.
It improves the pure blackness and color stability of the color material, forms a dense nanostructure, avoids color difference, and significantly improves the quality of the black color material.
Smart Images

Figure BDA0004750665180000031 
Figure BDA0004750665180000051 
Figure BDA0004750665180000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic pigments, and in particular relates to a method for preparing ceramic black pigment from waste steel slag. Background Art
[0002] Black ceramic pigment is a very important pigment in decorative materials. Black glaze is favored by people for its pure and solemn decorative effect, and is regarded as a treasure by high-end decoration companies. Every year, my country produces a large amount of toxic and harmful waste steel slag. These waste steel slags not only occupy a large area of open-air sites, but also pose a threat to human life and health. However, the copper, chromium, nickel and iron contained in the waste steel slag have important recycling value. If they can be recycled and made into black pigments, it will have very positive significance in all aspects. At present, there have been some reports on the preparation of black ceramic pigments using waste steel slag. For example, Chinese patent document CN101696125A discloses a method for preparing cobalt-free black ceramic pigment using copper tailings, and its technical solution is: copper tailings, iron oxide, chromium oxide, copper oxide, and nickel oxide are used as raw materials, mixed and calcined at 1180-1250°C for 1 hour, and the final product can be obtained after crushing; Chinese patent document CN102992808A discloses a method for preparing black ceramic pigment for blanks using chromium-containing waste slag, and its technical solution is: chromium-containing waste slag, iron oxide, and chromium oxide are used as raw materials, mixed and calcined at 1180-1250°C for 1 hour, and the final product can be obtained after crushing. However, the pigment product prepared by the above preparation method not only has a low blackness, but also has color difference, and the coloring is unstable, resulting in poor quality of the obtained black pigment. Summary of the invention
[0003] The invention discloses a method for preparing ceramic black pigment from waste steel slag, and belongs to the technical field of ceramic pigment. The preparation of black pigment comprises the following steps: soaking, filtering, washing, placing in deionized water and adjusting pH of waste steel slag, filtering and separating to obtain leachate; adjusting pH of leachate, adding sodium sulfide, filtering to obtain material slag A and material liquid B; mixing material slag A and sulfuric acid, controlling temperature to react, filtering to obtain material liquid C; mixing material liquid B and sodium chromate, adding sodium hydroxide, controlling temperature to react, filtering to obtain material slag D and material liquid E; mixing material slag D and dilute hydrochloric acid, adding material liquid C, deionized water, sodium bentonite, ultrasonic vibration, nitrogen filling and dropping potassium borohydride solution, stirring to obtain mixed liquid, vacuum drying to obtain support body; mixing support body and material liquid E, drying, calcining, grinding to obtain black pigment with high purity blackness effect.
[0004] The technical problem to be solved by the present invention is to produce a black colorant with relatively pure black chroma and stable coloring performance.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing ceramic black pigment from waste steel slag, the preparation of the black pigment comprising the following steps:
[0007] (1) soaking the waste steel slag, filtering, washing, removing impurities and dirt on the surface of the waste steel slag, placing it in deionized water and adjusting the pH, stirring, filtering and separating, so that copper, chromium, iron and nickel enter the leachate in the form of ions;
[0008] (2) adjusting the pH of the leaching solution, adding sodium sulfide, filtering, and obtaining a material slag A and a material liquid B; the material slag A comprises sulfides of copper and nickel; the material liquid B comprises ionic forms of iron and chromium; utilizing the difference in solubility products of metal sulfides to selectively precipitate copper and nickel, while retaining iron and chromium in the solution;
[0009] (3) mixing material slag A and sulfuric acid, controlling the temperature for reaction, filtering, and obtaining material liquid C; the material liquid C contains copper and nickel in ionic form; and hot pressing and leaching are performed so that the copper and nickel sulfides in the material slag A re-enter the solution in ionic form;
[0010] (4) taking material liquid B and sodium chromate, mixing and stirring, adding sodium hydroxide, controlling the temperature for reaction, filtering to obtain material slag D and material liquid E; the material slag D comprises iron red; the material liquid E comprises ion form of chromium; through hot pressing oxidation, the metal ions of chromium are oxidized into chromate ions and enter the solution, while the metal ions of iron are oxidized into iron red and separated;
[0011] (5) Mixing material slag D and dilute hydrochloric acid, adding material liquid C, deionized water, and sodium bentonite, ultrasonically vibrating, adding a potassium borohydride solution with strong reducing properties dropwise under nitrogen gas conditions, stirring to obtain a mixed solution, and vacuum drying to obtain a support;
[0012] (6) The support and the material liquid E are mixed, dried, calcined, and ground to obtain the black colorant.
[0013] As a preferred technical solution of the present invention, in step (3), the temperature-controlled reaction refers to stirring for 2-3 hours at 130-145°C and an oxygen partial pressure of 0.3-0.4 MPa.
[0014] As a preferred technical solution of the present invention, in step (4), the temperature-controlled reaction refers to stirring for 2-3 hours at 130-145°C and an oxygen partial pressure of 0.3-0.4 MPa.
[0015] As a preferred technical solution of the present invention, the leachate includes the following raw materials in parts by weight:
[0016]
[0017] As a preferred technical solution of the present invention, in step (2), the mass ratio of the leaching solution to sodium sulfide is 5-8:10-13.
[0018] As a preferred technical solution of the present invention, in step (3), the mass ratio of the material slag A to sulfuric acid is 1-3:20-30, and the concentration of the sulfuric acid is 10-12 mol / L.
[0019] As a preferred technical solution of the present invention, in step (4), the mass ratio of the material liquid B, sodium chromate and sodium hydroxide is 10-20:5-8:15-20.
[0020] As a preferred technical solution of the present invention, in step (5), the dosage ratio of the material slag D, dilute hydrochloric acid, material liquid C, deionized water, sodium bentonite, and potassium borohydride solution is 100-200g: 200-250mL: 50-60mL: 100mL: 20-25g: 500mL, the concentration of the potassium borohydride solution is 2-3mol / L; the concentration of the dilute hydrochloric acid is 2-4mol / L.
[0021] As a preferred technical solution of the present invention, in step (6), the mass ratio of the support body to the material liquid E is 4-6:50-80.
[0022] As a preferred technical solution of the present invention, in step (6), the calcination temperature is 1230-1280°C.
[0023] Beneficial effects of the present invention:
[0024] The method for preparing ceramic black pigment from waste steel slag disclosed in the present invention purifies the waste steel slag, thereby making the raw material used for preparing the black pigment purer and removing the adverse effects of impurities on chromaticity;
[0025] Furthermore, the iron / nickel and iron / copper supports loaded by sodium bentonite are complexed with chromium to form a nano-mixture, thereby preventing the migration of each coloring ion, so that the nano-scale spinel formed during the firing process is in a stable state, thereby improving the coloring stability;
[0026] Furthermore, the formation of nano-spinel has a denser structure and is less likely to reflect light, making the black color of the generated black pigment purer. DETAILED DESCRIPTION
[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0028] Example 1
[0029] A method for preparing ceramic black pigment from waste steel slag comprises the following steps:
[0030] (1) Take the waste steel slag and soak it, filter it, wash it, put it in a reactor, add 2L of deionized water and adjust the pH to 0.5, stir it for 2h, filter it and separate it, and obtain a leachate containing the following parts by weight of raw materials:
[0031]
[0032] (2) adjusting the pH of the leaching solution to 2.0, adding sodium sulfide, standing for 2 hours, filtering, and obtaining material slag A and material liquid B; the mass ratio of the leaching solution to sodium sulfide is 5:10;
[0033] (3) Mix material slag A and sulfuric acid, stir for 2 h at 130° C. and an oxygen partial pressure of 0.3 MPa, and filter to obtain material liquid C; the mass ratio of the material slag A to the sulfuric acid is 1:20, and the concentration of the sulfuric acid is 10 mol / L;
[0034] (4) Mixing material liquid B and sodium chromate, adding sodium hydroxide, stirring for 2 hours at 130° C. and an oxygen partial pressure of 0.3 MPa, and filtering to obtain material slag D and material liquid E; the mass ratio of the material liquid B, sodium chromate, and sodium hydroxide is 10:5:15;
[0035] (5) Take material slag D and dilute hydrochloric acid, mix and stir, add material liquid C, deionized water, and sodium bentonite, and vibrate ultrasonically for 20 minutes. Add potassium borohydride solution drop by drop under nitrogen filling conditions, stir for 2 hours to obtain a mixed solution, and vacuum dry for 24 hours to obtain a support; the dosage ratio of the material slag D, dilute hydrochloric acid, material liquid C, deionized water, sodium bentonite, and potassium borohydride solution is 100g:200mL:50mL:100mL:20g:500mL, the concentration of the potassium borohydride solution is 2mol / L; the concentration of the dilute hydrochloric acid is 2mol / L;
[0036] (6) The support body and the material liquid E are mixed and stirred for 1 hour, dried, calcined at 1230° C. for 5 hours, and ground to obtain the black colorant; the mass ratio of the support body to the material liquid E is 4:50.
[0037] Example 2
[0038] A method for preparing ceramic black pigment from waste steel slag comprises the following steps:
[0039] (1) Take the waste steel slag, soak it, filter it, wash it, put it in a reactor, add 2L of deionized water and adjust the pH to 0.8, stir it for 2.5h, filter it and separate it, and obtain a leachate containing the following parts by weight of raw materials:
[0040]
[0041] (2) adjusting the pH of the leaching solution to 2.2, adding sodium sulfide, standing for 2.5 hours, filtering, and obtaining material slag A and material liquid B; the mass ratio of the leaching solution to sodium sulfide is 7:12;
[0042] (3) Mix material slag A and sulfuric acid, stir for 2.5 hours at 140° C. and an oxygen partial pressure of 0.35 MPa, and filter to obtain material liquid C; the mass ratio of the material slag A to the sulfuric acid is 2:25, and the concentration of the sulfuric acid is 11 mol / L;
[0043] (4) Mixing material liquid B and sodium chromate, adding sodium hydroxide, stirring for 2.5 hours at 140° C. and an oxygen partial pressure of 0.35 MPa, and filtering to obtain material slag D and material liquid E; the mass ratio of the material liquid B, sodium chromate, and sodium hydroxide is 15:6:17;
[0044] (5) Take material slag D and dilute hydrochloric acid, mix and stir, add material liquid C, deionized water, and sodium bentonite, and vibrate ultrasonically for 30 minutes. Add potassium borohydride solution drop by drop under nitrogen filling conditions, stir for 2.5 hours to obtain a mixed solution, and vacuum dry for 24 hours to obtain a support; the dosage ratio of the material slag D, dilute hydrochloric acid, material liquid C, deionized water, sodium bentonite, and potassium borohydride solution is 150g:225mL:55mL:100mL:22g:500mL, the concentration of the potassium borohydride solution is 2.5mol / L; the concentration of the dilute hydrochloric acid is 3mol / L;
[0045] (6) The support and the material liquid E are mixed and stirred for 1.5 hours, dried, calcined at 1250° C. for 6 hours, and ground to obtain the black colorant; the mass ratio of the support and the material liquid E is 5:60.
[0046] Example 3
[0047] A method for preparing ceramic black pigment from waste steel slag comprises the following steps:
[0048] (1) Take the waste steel slag, soak it, filter it, wash it, put it in a reactor, add 2L of deionized water and adjust the pH to 1.0, stir it for 3h, filter it and separate it, and obtain a leachate containing the following parts by weight of raw materials:
[0049]
[0050] (2) adjusting the pH of the leaching solution to 2.5, adding sodium sulfide, standing for 3 hours, filtering, and obtaining material slag A and material liquid B; the mass ratio of the leaching solution to sodium sulfide is 8:13;
[0051] (3) Mix material slag A and sulfuric acid, stir for 3 hours at 145° C. and an oxygen partial pressure of 0.4 MPa, and filter to obtain material liquid C; the mass ratio of the material slag A to the sulfuric acid is 3:30, and the concentration of the sulfuric acid is 12 mol / L;
[0052] (4) Mixing material liquid B and sodium chromate, adding sodium hydroxide, stirring for 3 hours at 145° C. and an oxygen partial pressure of 0.4 MPa, and filtering to obtain material slag D and material liquid E; the mass ratio of the material liquid B, sodium chromate, and sodium hydroxide is 20:8:20;
[0053] (5) Take material slag D and dilute hydrochloric acid, mix and stir, add material liquid C, deionized water, and sodium bentonite, and ultrasonically vibrate for 40 minutes. Under nitrogen filling conditions, potassium borohydride solution is added dropwise, stirred for 3 hours to obtain a mixed solution, and vacuum dried for 24 hours to obtain a support; the dosage ratio of the material slag D, dilute hydrochloric acid, material liquid C, deionized water, sodium bentonite, and potassium borohydride solution is 200g:250mL:60mL:100mL:25g:500mL, the concentration of the potassium borohydride solution is 3mol / L; the concentration of the dilute hydrochloric acid is 4mol / L;
[0054] (6) The support body and the material liquid E are mixed and stirred for 2 hours, dried, calcined at 1280° C. for 8 hours, and ground to obtain the black colorant; the mass ratio of the support body to the material liquid E is 6:80.
[0055] Comparative Example 1
[0056] A method for preparing ceramic black pigment from waste steel slag comprises the following steps:
[0057] (1) Take the waste steel slag and soak it, filter it, wash it, put it in a reactor, add 2L of deionized water and adjust the pH to 0.5, stir it for 2h, filter it and separate it, and obtain a leachate containing the following parts by weight of raw materials:
[0058]
[0059] (2) adjusting the pH of the leaching solution to 2.0, adding sodium sulfide, standing for 2 hours, filtering, and obtaining material slag A and material liquid B; the mass ratio of the leaching solution to sodium sulfide is 5:10;
[0060] (3) Mix material slag A and sulfuric acid, stir for 2 h at 130° C. and an oxygen partial pressure of 0.3 MPa, and filter to obtain material liquid C; the mass ratio of the material slag A to the sulfuric acid is 1:20, and the concentration of the sulfuric acid is 10 mol / L;
[0061] (4) Mixing material liquid B and sodium chromate, adding sodium hydroxide, stirring for 2 hours at 130° C. and an oxygen partial pressure of 0.3 MPa, and filtering to obtain material slag D and material liquid E; the mass ratio of the material liquid B, sodium chromate, and sodium hydroxide is 10:5:15;
[0062] (5) Take material slag D and dilute hydrochloric acid, mix and stir, add material liquid C and deionized water, and oscillate ultrasonically for 20 minutes. Add potassium borohydride solution drop by drop under nitrogen filling conditions, stir for 2 hours to obtain a mixed solution, and vacuum dry for 24 hours to obtain a mixed material; the dosage ratio of the material slag D, dilute hydrochloric acid, material liquid C, deionized water, and potassium borohydride solution is 100g:200mL:50mL:100mL:500mL, the concentration of the potassium borohydride solution is 2mol / L; the concentration of the dilute hydrochloric acid is 2mol / L;
[0063] (6) The mixed material and liquid E are mixed and stirred for 1 hour, dried, calcined at 1230° C. for 5 hours, and ground to obtain the black colorant; the mass ratio of the mixed material to liquid E is 4:50.
[0064] Performance Testing
[0065] The WSD-3C fully automatic whiteness meter produced by Beijing Kangguang Instrument Co., Ltd. was used to measure the L*, a*, and b* values of the black colorants prepared in Examples 1-3. The results are shown in Table 1 below.
[0066] Table 1
[0067] L* a* b* Appearance Color Example 1 16.86 0.81 0.85 black Example 2 16.91 0.84 0.92 black Example 3 16.81 0.85 0.87 black Comparative Example 1 19.32 1.89 2.21 Dark brown
[0068] As can be seen from Table 1, the black colorants prepared in Examples 1-3 have a relatively pure black degree and stable color development performance. Comparative Example 1 is prepared on the basis of Example 1, and its black degree is obviously impure compared with Example 1.
[0069] Note: The waste steel slag involved in the present invention was purchased from Qian'an Iron and Steel Company of Shougang Group Co., Ltd., and the sodium-based bentonite was purchased from Wuhan Kanos Technology Co., Ltd.
[0070] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing ceramic black pigment from waste steel slag, characterized in that: The preparation of the black colorant comprises the following steps: (1) soaking the waste steel slag, filtering, washing, placing in deionized water and adjusting the pH, stirring, filtering and separating to obtain a leachate; (2) adjusting the pH of the leaching solution, adding sodium sulfide, filtering, and obtaining material slag A and material liquid B; (3) Mix material slag A and sulfuric acid, control the temperature for reaction, filter, and obtain material liquid C; (4) Mix material liquid B and sodium chromate, add sodium hydroxide, control the temperature to react, and filter to obtain material slag D and material liquid E; (5) Take the material slag D and dilute hydrochloric acid, mix and stir, add the material liquid C, deionized water, and sodium bentonite, add potassium borohydride solution drop by drop under ultrasonic vibration and nitrogen filling, stir to obtain a mixed solution, and vacuum dry to obtain a support; (6) Mixing the support and the material liquid E, drying, calcining, and grinding to obtain the black colorant; In step (3), the temperature-controlled reaction refers to stirring for 2-3 hours at 130-145°C and an oxygen partial pressure of 0.3-0.4 MPa; In step (4), the temperature-controlled reaction refers to stirring for 2-3 hours at 130-145°C and an oxygen partial pressure of 0.3-0.4 MPa; The leachate includes the following raw materials in parts by weight: 22-32 parts by weight of iron Copper element 11-15 parts by mass Chromium 14-18 parts by mass 7-10 parts by mass of nickel; In step (2), the mass ratio of the leaching solution to sodium sulfide is 5-8:10-13; In step (3), the mass ratio of the material slag A to sulfuric acid is 1-3:20-30, and the concentration of the sulfuric acid is 10-12 mol / L; In step (4), the mass ratio of the material liquid B, sodium chromate and sodium hydroxide is 10-20:5-8:15-20; In step (5), the dosage ratio of the material slag D, dilute hydrochloric acid, material liquid C, deionized water, sodium bentonite, and potassium borohydride solution is 100-200 g: 200-250 mL: 50-60 mL: 100 mL: 20-25 g: 500 mL, the concentration of the potassium borohydride solution is 2-3 mol / L; the concentration of the dilute hydrochloric acid is 2-4 mol / L; In step (6), the mass ratio of the support body to the feed liquid E is 4-6:50-80; In step (6), the calcination temperature is 1230-1280°C.