A thermally conductive copper-based electromagnetic shielding material and its synthesis process
Through copper-based electromagnetic shielding material composed of carbon nanotube-cobalt nanoparticles wrapped by copper and ABS resin, the problems of poor shielding effect and insufficient thermal conductivity in the existing technology are solved, and efficient absorption and attenuation of electromagnetic waves are achieved effect.
Patent Information
- Application Number
- CN202211193553.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-28
AI Technical Summary
The existing electromagnetic shielding materials have poor shielding effects at both high-frequency and low-frequency electromagnetic fields, and are insufficient in thermal conductivity and heat dissipation, making it difficult to effectively absorb and attenuate electromagnetic waves.
The copper-based electromagnetic shielding material consisting of inner white copper and outer ABS resin wrapped in carbon nanotube-cobalt nanoparticles was prepared through the flat vulcanizer molding process. The ABS resin and carbon nanotube-cobalt nanoparticles were melt blended. Cobalt nanoparticles grow uniformly on the surface of carbon nanotubes, enhancing interface polarization effect and impedance matching, and improving electromagnetic wave absorption and attenuation performance.
The copper-based electromagnetic shielding material with strong thermal conductivity and heat dissipation is realized, which can effectively absorb and attenuate electromagnetic waves within a wide frequency range, improve electromagnetic shielding performance, and promote the dissipation of electromagnetic waves in the form of thermal energy.
Smart Images

Figure CN115352147B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding, in particular to a thermally conductive copper-based electromagnetic shielding material and a synthesis process thereof. Background Art
[0002] Electromagnetic shielding materials are widely used in anti-electromagnetic pollution, electronic and electrical components, stealth technology, etc.; currently, there are very high technical requirements for electromagnetic shielding materials. When the frequency of the interfering electromagnetic field is high, low resistivity metal materials can be used to achieve electromagnetic shielding effects; when the frequency of the interfering electromagnetic wave is low, high magnetic permeability materials are needed to prevent it from spreading to the shielded space.
[0003] The use of different metal materials to form a multi-layer shield can have a shielding effect on both high-frequency and low-frequency electromagnetic fields; for example, the paper "Preparation of Graphene / Magnetic Particles / Resin-based Composite Materials and Study on Electromagnetic Shielding Performance" discloses that graphene and magnetic particles are simultaneously filled into an acrylonitrile-butadiene-styrene copolymer (ABS resin) matrix, and a small amount of nickel-plated carbon fiber is added, which has good electromagnetic shielding performance. Carbon nanotubes have strong electrical and thermal conductivity and excellent electromagnetic shielding performance, and have broad application prospects in electromagnetic shielding materials. For example, the document "Study on the Electromagnetic Shielding Performance of Metal-coated Carbon Nanotubes" reports that after acidification, sensitization and activation treatment, carbon nanotubes are prepared by ultrasonic spray chemical plating, and then nickel-plated copper carbon nanotubes and nickel-plated silver carbon nanotubes are prepared by molecular-level blending. Composite materials have excellent electromagnetic shielding performance. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The invention provides a copper-based electromagnetic shielding material with good thermal conductivity and heat dissipation and excellent electromagnetic shielding performance and a synthesis process thereof.
[0006] (II) Technical solution
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a thermally conductive copper-based electromagnetic shielding material, characterized in that the thermally conductive copper-based electromagnetic shielding material is composed of an inner layer of nickel silver and an outer layer of ABS (acrylonitrile-butadiene-styrene copolymer) resin wrapped with carbon nanotubes-cobalt nanoparticles.
[0008] Preferably, the synthesis process is: using nickel silver with a thickness of 0.2-0.8 mm as the middle layer, and molding the carbon nanotube-cobalt nanoparticles wrapped with ABS resin on the entire outer layer of the nickel silver through a flat vulcanizer, with a thickness of 2-3 mm, to obtain a thermally conductive copper-based electromagnetic shielding material.
[0009] Preferably, the molding temperature is 200-220° C., the pressure is 6-10 MPa, and the molding time is 5-10 min.
[0010] Preferably, the synthesis process of the ABS resin-wrapped carbon nanotube-cobalt nanoparticles is:
[0011] (1) 100 parts by weight of hydroxylated carbon nanotubes are uniformly dispersed in a reaction solvent, 300-800 parts by weight of chloroacetyl chloride and 120-300 parts by weight of triethylamine are added, and the mixture is reacted at 15-30° C. for 6-18 hours. The solvent is filtered, and the mixture is washed with ethanol to obtain chloroacetic acid esterified carbon nanotubes.
[0012] (2) Add 250-600 parts by weight of L-aspartic acid and 60-150 parts by weight of a catalyst to 100 parts by weight of chloroacetic acid esterified carbon nanotubes in N,N-dimethylformamide, and react at 50-75°C for 6-12 hours. After the reaction, add dilute hydrochloric acid to adjust the pH to 4-5, filter the solvent, and wash with deionized water to obtain dibutyric acid imide carbon nanotubes.
[0013] (3) Disperse 100 parts by weight of dibutyric acid imide carbon nanoparticles and 15-50 parts by weight of cobalt dichloride uniformly in deionized water, stir for 3-8 hours, then add 30-120 parts by weight of potassium borohydride, react at 0-10 ° C in a nitrogen atmosphere for 1-4 hours, filter the solvent, wash with deionized water, and obtain carbon nanotube-loaded cobalt nanoparticles.
[0014] (4) Add ABS resin and carbon nanotube-loaded cobalt nanoparticles into a torque rheometer and melt-blend them at 160-180 °C for 5-10 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
[0015] Preferably, the reaction solvent in (1) comprises acetonitrile, dichloromethane, chloroform, acetone, tetrahydrofuran, or ethyl acetate.
[0016] Preferably, the catalyst in (2) comprises sodium hydroxide or potassium hydroxide.
[0017] Preferably, the amount of carbon nanotubes loaded with cobalt nanoparticles in (4) is 1-8% by weight of the ABS resin.
[0018] 3. Beneficial technical effects
[0019] Compared with the prior art, the present invention has the following beneficial technical effects:
[0020] Chloroacetyl chloride is used to react with hydroxylated carbon nanotubes to undergo an esterification reaction to obtain chloroacetic acid esterified carbon nanotubes, and then the chlorine atom undergoes a substitution reaction with the amino group of L-aspartic acid to obtain dibutyric acid imide carbon nanotubes, thereby modifying the dibutyric acid imino groups on the surface of the carbon nanotubes.
[0021] Using dibutyric acid imino groups modified on the surface of carbon nanotubes to synthesize Co 2+ To carry out coordination complexation, Co 2+ The Co is uniformly loaded onto the surface of carbon nanotubes with high specific surface area, and then reduced by potassium borohydride. 2+ Cobalt nanoparticles are generated so that the cobalt nanoparticles grow evenly on the surface of the carbon nanotubes, thereby reducing the agglomeration of the cobalt nanoparticles.
[0022] Carbon nanotubes loaded with cobalt nanoparticles and ABS resin are melt-blended and then used as the outer layer, and nickel silver is used as the inner layer. The resin is pressed onto the surface of the inner nickel silver layer to obtain a copper-based electromagnetic shielding material. The cobalt nanoparticles grow uniformly on the surface of the carbon nanotubes, and there is a better interface polarization effect and impedance matching between the two, and the absorption and attenuation performance of electromagnetic waves is better. The nickel silver inner layer and the carbon nanotubes loaded with cobalt nanoparticles have high thermal conductivity. The obtained copper-based electromagnetic shielding material has strong thermal conductivity and heat dissipation, which can promote the dissipation of absorbed electromagnetic waves in the form of heat energy, thereby improving the electromagnetic shielding performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a table of electromagnetic shielding performance of the samples in the present invention.
[0024] Figure 2 It is a thermal conductivity test table of the copper-based electromagnetic shielding material in the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the attached embodiment of the present invention Figure 1-2 , the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] (1) 100 parts by weight of hydroxylated carbon nanotubes were uniformly dispersed in dichloromethane, 380 parts by weight of chloroacetyl chloride and 150 parts by weight of triethylamine were added, and the mixture was reacted at 20°C for 18 h. The solvent was filtered and washed with ethanol to obtain chloroacetic acid esterified carbon nanotubes.
[0028] (2) Add 250 parts by weight of L-aspartic acid and 60 parts by weight of sodium hydroxide catalyst to 100 parts by weight of chloroacetic acid esterified carbon nanotubes in N,N-dimethylformamide, and react at 50°C for 12 h. After the reaction, add dilute hydrochloric acid to adjust the pH to 5, filter the solvent, and wash with deionized water to obtain dibutyric acid imide carbon nanotubes.
[0029] (3) 100 parts by weight of dibutyric acid imide carbon nanoparticles and 15 parts by weight of cobalt dichloride were uniformly dispersed in deionized water and stirred for 8 h. Then 30 parts by weight of potassium borohydride were added and reacted at 0 °C in a nitrogen atmosphere for 2 h. The solvent was filtered and washed with deionized water to obtain carbon nanotube-loaded cobalt nanoparticles.
[0030] (4) 100 parts by weight of ABS resin and 1 part by weight of carbon nanotube-loaded cobalt nanoparticles were added to a torque rheometer and melt-blended at 180°C for 5 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
[0031] (5) A 0.4 mm thick nickel silver was used as the middle layer, and ABS resin-wrapped carbon nanotube-cobalt nanoparticles were molded on the entire outer layer of the nickel silver through a flat vulcanizer with a thickness of 3 mm. The molding temperature was controlled at 210 °C, the pressure was 8 MPa, and the molding time was 5 min to obtain a thermally conductive copper-based electromagnetic shielding material.
[0032] Example 2
[0033] (1) 100 parts by weight of hydroxylated carbon nanotubes were uniformly dispersed in acetone, 300 parts by weight of chloroacetyl chloride and 120 parts by weight of triethylamine were added, and the mixture was reacted at 20°C for 12 h. The solvent was filtered and washed with ethanol to obtain chloroacetic acid esterified carbon nanotubes.
[0034] (2) 350 parts by weight of L-aspartic acid and 80 parts by weight of potassium hydroxide catalyst were added to 100 parts by weight of chloroacetic acid esterified carbon nanotubes in N,N-dimethylformamide, and the mixture was reacted at 65°C for 12 h. After the reaction, dilute hydrochloric acid was added dropwise to adjust the pH to 4, the solvent was filtered, and the mixture was washed with deionized water to obtain dibutyric acid imide carbon nanotubes.
[0035] (3) 100 parts by weight of dibutyric acid imide carbon nanoparticles and 15 parts by weight of cobalt dichloride were uniformly dispersed in deionized water and stirred for 4 h. Then, 30 parts by weight of potassium borohydride were added and reacted at 5 °C in a nitrogen atmosphere for 2 h. The solvent was filtered and washed with deionized water to obtain carbon nanotube-loaded cobalt nanoparticles.
[0036] (4) 100 parts by weight of ABS resin and 3 parts by weight of carbon nanotube-loaded cobalt nanoparticles were added to a torque rheometer and melt-blended at 170 °C for 8 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
[0037] (5) A 0.5 mm thick nickel silver was used as the middle layer, and ABS resin-wrapped carbon nanotube-cobalt nanoparticles were molded on the entire outer layer of the nickel silver through a flat vulcanizer with a thickness of 3 mm. The molding temperature was controlled at 200 °C, the pressure was 10 MPa, and the molding time was 10 min to obtain a thermally conductive copper-based electromagnetic shielding material.
[0038] Example 3
[0039] (1) 100 parts by weight of hydroxylated carbon nanotubes were uniformly dispersed in ethyl acetate, 620 parts by weight of chloroacetyl chloride and 250 parts by weight of triethylamine were added, and the mixture was reacted at 30°C for 12 h. The solvent was filtered and washed with ethanol to obtain chloroacetic acid esterified carbon nanotubes.
[0040] (2) 380 parts by weight of L-aspartic acid and 120 parts by weight of sodium hydroxide catalyst were added to 100 parts by weight of chloroacetic acid esterified carbon nanotubes in N,N-dimethylformamide, and the mixture was reacted at 75°C for 6 h. After the reaction, dilute hydrochloric acid was added dropwise to adjust the pH to 5, the solvent was filtered, and the mixture was washed with deionized water to obtain dibutyric acid imide carbon nanotubes.
[0041] (3) 100 parts by weight of dibutyric acid imide carbon nanoparticles and 50 parts by weight of cobalt dichloride were uniformly dispersed in deionized water and stirred for 8 h. Then, 120 parts by weight of potassium borohydride were added and reacted at 10 °C in a nitrogen atmosphere for 2 h. The solvent was filtered and washed with deionized water to obtain carbon nanotube-loaded cobalt nanoparticles.
[0042] (4) 100 parts by weight of ABS resin and 6 parts by weight of carbon nanotube-loaded cobalt nanoparticles were added to a torque rheometer and melt-blended at 160 °C for 8 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
[0043] (5) A 0.8 mm thick nickel silver was used as the middle layer, and ABS resin-wrapped carbon nanotube-cobalt nanoparticles were molded on the entire outer layer of the nickel silver through a flat vulcanizer with a thickness of 3 mm. The molding temperature was controlled at 220 °C, the pressure was 6 MPa, and the molding time was 10 min to obtain a thermally conductive copper-based electromagnetic shielding material.
[0044] Example 4
[0045] (1) 100 parts by weight of hydroxylated carbon nanotubes were uniformly dispersed in acetonitrile, 800 parts by weight of chloroacetyl chloride and 300 parts by weight of triethylamine were added, and the mixture was reacted at 30°C for 6 h. The solvent was filtered and washed with ethanol to obtain chloroacetic acid esterified carbon nanotubes.
[0046] (2) 600 parts by weight of L-aspartic acid and 150 parts by weight of potassium hydroxide catalyst were added to 100 parts by weight of chloroacetic acid esterified carbon nanotubes in N,N-dimethylformamide, and the mixture was reacted at 50°C for 6 h. After the reaction, dilute hydrochloric acid was added dropwise to adjust the pH to 5, the solvent was filtered, and the mixture was washed with deionized water to obtain dibutyric acid imide carbon nanotubes.
[0047] (3) 100 parts by weight of dibutyric acid imide carbon nanoparticles and 40 parts by weight of cobalt dichloride were uniformly dispersed in deionized water and stirred for 6 h. Then, 100 parts by weight of potassium borohydride were added and reacted at 5 °C in a nitrogen atmosphere for 2 h. The solvent was filtered and washed with deionized water to obtain carbon nanotube-loaded cobalt nanoparticles.
[0048] (4) 100 parts by weight of ABS resin and 8 parts by weight of carbon nanotube-loaded cobalt nanoparticles were added to a torque rheometer and melt-blended at 170 °C for 10 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
[0049] (5) A 0.8 mm thick nickel silver was used as the middle layer, and ABS resin-wrapped carbon nanotube-cobalt nanoparticles were molded on the entire outer layer of the nickel silver through a flat vulcanizer with a thickness of 2 mm. The molding temperature was controlled at 220 °C, the pressure was 6 MPa, and the molding time was 10 min to obtain a thermally conductive copper-based electromagnetic shielding material.
[0050] Comparative Example 1
[0051] (1) 100 parts by weight of ABS resin and 1 part by weight of carbon nanotubes were added into a torque rheometer and melt-blended at 170 °C for 10 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
[0052] (2) A 0.2 mm thick nickel silver was used as the middle layer, and ABS resin-wrapped carbon nanotube-cobalt nanoparticles were molded on the entire outer layer of the nickel silver through a flat vulcanizer with a thickness of 3 mm. The molding temperature was controlled at 220 °C, the pressure was 8 MPa, and the molding time was 6 min to obtain a thermally conductive copper-based electromagnetic shielding material.
[0053] Comparative Example 2
[0054] (1) 100 parts by weight of ABS resin, 1 part by weight of carbon nanotubes, and 0.2 parts by weight of cobalt nanoparticles were added to a torque rheometer and melt-blended at 170°C for 5 min to obtain ABS resin-wrapped carbon nanotubes-cobalt nanoparticles.
[0055] (2) A 0.2 mm thick nickel silver was used as the middle layer, and ABS resin-wrapped carbon nanotube-cobalt nanoparticles were molded on the entire outer layer of the nickel silver through a flat vulcanizer with a thickness of 3 mm. The molding temperature was controlled at 200 °C, the pressure was 8 MPa, and the molding time was 10 min to obtain a thermally conductive copper-based electromagnetic shielding material.
[0056] The copper-based electromagnetic shielding material was cut into rings with an inner diameter of 2 mm and an outer diameter of 5 mm. The electromagnetic shielding performance of the sample was tested by a vector network analyzer with a test frequency range of 1-100 GHz.
[0057] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 ≦-20db absorption frequency (GHz) 8.1-13.5 7.6-13.2 7.9-14.0 7.7-13.0 8.9-10.8 8.6-12.1 Maximum absorption loss (db) -32.4 -40.6 -36.9 -35.1 -21.4 -30.1
[0058] The thermal conductivity of the copper-based electromagnetic shielding material was then measured using a thermal conductivity tester, with a sample length of 10 cm and a width of 3 cm.
[0059] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Thermal conductivity (W / (m·k)) 6.94 7.30 6.29 6.63 5.64 6.13
[0060] After the electromagnetic shielding performance test, the copper-based electromagnetic shielding material has an absorption frequency of ≦-20db, with a maximum absorption loss of -40.6db.
[0061] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A thermally conductive copper-based electromagnetic shielding material, characterized in that: The thermally conductive copper-based electromagnetic shielding material is composed of an inner layer of nickel silver and an outer layer of ABS resin wrapped with carbon nanotube-cobalt nanoparticles; The synthesis process of the thermally conductive copper-based electromagnetic shielding material is as follows: nickel silver with a thickness of 0.2-0.8 mm is used as an intermediate layer, and carbon nanotube-cobalt nanoparticles wrapped with ABS resin are molded on the entire outer layer of the nickel silver through a flat vulcanizer, with a thickness of 2-3 mm, to obtain a thermally conductive copper-based electromagnetic shielding material; The synthesis process of the ABS resin-wrapped carbon nanotube-cobalt nanoparticles is as follows: (1) Dispersing 100 parts by weight of hydroxylated carbon nanotubes uniformly in a reaction solvent, adding 300-800 parts by weight of chloroacetyl chloride and 120-300 parts by weight of triethylamine, reacting at 15-30° C. for 6-18 hours, filtering the solvent, washing with ethanol, and obtaining chloroacetic acid esterified carbon nanotubes; (2) adding 250-600 parts by weight of L-aspartic acid and 60-150 parts by weight of a catalyst to 100 parts by weight of chloroacetic acid esterified carbon nanotubes in N,N-dimethylformamide, reacting at 50-75°C for 6-12 hours, adding dilute hydrochloric acid to adjust the pH to 4-5 after the reaction, filtering the solvent, and washing with deionized water to obtain dibutyric acid iminated carbon nanotubes; (3) Dispersing 100 parts by weight of dibutyric acid imide carbon nanotubes and 15-50 parts by weight of cobalt dichloride uniformly in deionized water, stirring for 3-8 hours, then adding 30-120 parts by weight of potassium borohydride, reacting at 0-10°C in a nitrogen atmosphere for 1-4 hours, filtering the solvent, and washing with deionized water to obtain carbon nanotube-loaded cobalt nanoparticles; (4) Add ABS resin and carbon nanotube-loaded cobalt nanoparticles into a torque rheometer and melt-blend them at 160-180 °C for 5-10 min to obtain ABS resin-wrapped carbon nanotube-cobalt nanoparticles.
2. The synthesis process of the thermally conductive copper-based electromagnetic shielding material according to claim 1, characterized in that: The molding temperature is 200-220°C, the pressure is 6-10 MPa, and the molding time is 5-10 min.
3. The synthesis process of the thermally conductive copper-based electromagnetic shielding material according to claim 1, characterized in that: The reaction solvent in (1) includes acetonitrile, dichloromethane, chloroform, acetone, tetrahydrofuran, and ethyl acetate.
4. The synthesis process of the thermally conductive copper-based electromagnetic shielding material according to claim 1, characterized in that: The catalyst in (2) includes sodium hydroxide and potassium hydroxide.
5. The synthesis process of the thermally conductive copper-based electromagnetic shielding material according to claim 1, characterized in that: The amount of carbon nanotubes loaded with cobalt nanoparticles in (4) is 1-8% by weight of the ABS resin.