A method for preparing non-shrinkable polyacrylic acid film
By introducing graphene oxide and multivalent iron ions into the polyacrylic acid film, and stretching and heat setting twice, a stable hydrogen bond and coordination cross-linked network is formed, which solves the problem of dimensional shrinkage and poor performance of the polyacrylic acid film. problem, achieving film preparation with non-shrinkability and high iron ion loading rate.
Patent Information
- Application Number
- CN202410692666.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-31
AI Technical Summary
Traditional polyacrylic acid films have dimensional shrinkage problems, resulting in reduced specific surface area, poor mechanical properties, insufficient water resistance and low iron ion loading capacity. It is difficult to prepare non-shrinkable polyacrylic acid films using existing methods.
After extruding the film-making solution into a film using a film maker, it is soaked in a coagulation bath, and stretched and heat-set twice. Graphene oxide and multivalent iron ions are used to form stable hydrogen bonds and coordination interactions. The network is connected to control the movement and changes of polyacrylic acid macromolecular chains to prepare a non-shrinkable polyacrylic acid film.
The non-shrinkability of the polyacrylic acid film is achieved, its mechanical properties, water resistance and iron ion loading rate are improved, the stability of the specific surface area is maintained, the iron ion leaching rate is reduced, and the catalytic activity is enhanced.
Smart Images

Figure SMS_9
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of films and relates to a method for preparing a non-shrinkable polyacrylic acid film. Background Art
[0002] In recent years, with the rapid development of film industry technology, film forming and processing technology has gradually matured. Most of the films currently produced have met people's basic usage requirements, but in the face of increasing market demand, it is very necessary to optimize the structure and improve the performance of the film.
[0003] Traditional polyacrylic acid films generally have the problem of large dimensional shrinkage, which can lead to a significant reduction in the specific surface area of the film material, poor mechanical properties, insufficient water resistance, and low iron ion loading and fixation capacity.
[0004] In order to solve the above problems, CN109504012A provides a method for preparing a graphene oxide-polyacrylic acid imitation shell mother-of-pearl layered composite film. The prepared graphene oxide-polyacrylic acid imitation shell mother-of-pearl layered composite film has strong mechanical properties and good structural stability. However, due to the random orientation of polyacrylic acid, the layered orientation of the film material is weak and the layered structure is unstable. The shrinkage rate of the prepared film material cannot be significantly reduced, and the preparation process is cumbersome, so it is impossible to prepare a non-shrinkable polyacrylic acid film.
[0005] Therefore, it is of great significance to study a method for preparing a non-shrinkable polyacrylic acid film to solve the above problems. Summary of the invention
[0006] The purpose of the invention is to solve the problems existing in the prior art and provide a method for preparing a non-shrinkable polyacrylic acid film.
[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a non-shrinkable polyacrylic acid film comprises: using a film-making device to extrude a film-making solution into a film, immersing the film in a coagulation bath, taking out the film, sequentially stretching and heat-setting the film to obtain a primary-stretched film, and finally immersing the primary-stretched film in a coagulation bath, taking it out, and sequentially stretching and heat-setting the film to obtain a non-shrinkable polyacrylic acid film.
[0009] The membrane-making solution is composed of polyacrylic acid, formamide, water and graphene oxide, and the added amount of graphene oxide is 0.25-2.0wt% of the polyacrylic acid;
[0010] The polyacrylic acid is a copolymer of maleic anhydride and acrylic acid;
[0011] The coagulation bath contains Fe 2+ and Fe 3+ When the iron ions in the coagulation bath are in mixed valence state, due to Fe 2+ and Fe 3+ The spin states are different, and the effective ionic radius is Fe 2+ >Fe 3+ Therefore, the bond strength between the iron ion and the carboxyl group is Fe 3+ >Fe 2+ In this case, Fe 2+ and Fe 3+ They will form loose and changeable coordination cross-linking networks and dense and stable coordination cross-linking networks with polyacrylic acid macromolecule chains respectively, while mixed-valence iron ions will form moderately ordered coordination cross-linking networks with polyacrylic acid macromolecule chains. Compared with polyacrylic acid fibers coordinated by monovalent iron ions, polyacrylic acid fibers coordinated by mixed-valence iron ions can withstand higher stretching times and higher temperature heat setting.
[0012] The shrinkage rate of the non-shrinkable polyacrylic acid film when immersed in water at 25° C. for 10 minutes is 0.
[0013] As the preferred technical solution:
[0014] The method for preparing a non-shrinkable polyacrylic acid film as described above, wherein the specific surface area of the non-shrinkable polyacrylic acid film is 51.49×10 -3 ~69.87×10 -3 m 2 / mg, the dissolution rate after immersion in 85℃ water for 4h was 21.48~27.68%, the catalytic activity was 3~7min, the iron ion loading rate was 8.47~11.29%, and the iron ion leaching rate was 13.67~69.78%.
[0015] In the method for preparing a non-shrinkable polyacrylic acid film as described above, the mass ratio of polyacrylic acid, formamide and water in the film-making solution is 3.0:2.7~10.8:16.2~24.3.
[0016] The method for preparing a non-shrinkable polyacrylic acid film as described above, wherein the polyacrylic acid is obtained by free radical polymerization of acrylic acid and maleic anhydride in a mass ratio of 95:5 under the action of benzoyl peroxide, the polymerization time is 2.5 hours, the polymerization temperature is 85°C, and the stirring speed during polymerization is 180r / min.
[0017] In the method for preparing a non-shrinkable polyacrylic acid film as described above, the coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:4.12-5.49:10.10-11.78.
[0018] In the preparation method of a non-shrinkable polyacrylic acid film as described above, the first immersion treatment time in the coagulation bath is 4 hours, the first stretching multiple is 16 to 20 times (the first stretching is performed at room temperature), and the first heat setting condition is: setting at a temperature of 60 to 140°C for 0.5 to 12 hours.
[0019] In the preparation method of a non-shrinkable polyacrylic acid film as described above, the second immersion treatment time in the coagulation bath is 4 hours, the second stretching multiple is 1.4~1.5 (the second stretching is carried out at room temperature), and the second heat setting conditions are: setting at a temperature of 60~140°C for 0.5~12 hours.
[0020] Principle of the invention:
[0021] In the present invention, a non-shrinkable polyacrylic acid film is prepared by combining polyacrylic acid, graphene oxide and iron ions and then stretching them twice;
[0022] Among them, a small amount of coordinated cross-linked network structure is formed between the hydroxyl and carboxyl groups on graphene oxide and the iron ions, that is, the interaction force between graphene oxide and iron ions is formed to assist in stabilizing the structure of the film; a large number of hydrogen bonds are formed between the hydroxyl and carboxyl groups on graphene oxide and the polyacrylic acid macromolecule chain, that is, the interaction force between the graphene oxide sheet and polyacrylic acid is formed to fix the structural size of the film; coordination bonds are formed between iron ions and polyacrylic acid macromolecule chains, that is, the interaction force between polyacrylic acid macromolecule chains and iron ions is formed to stabilize the basic structural morphology of the film. The existence of these three different interaction forces effectively controls the movement and changes of polyacrylic acid macromolecule chains and stabilizes the internal structure of polyacrylic acid film.
[0023] The secondary stretching peels off the multilayer graphene oxide sheets into single-layer graphene oxide sheets. The hydrogen bonding between the dispersed single-layer graphene oxide sheets and the fully stretched polyacrylic acid macromolecular chains can more effectively fix the structural dimensions of the film, which plays a key role in the non-shrinkability of the film.
[0024] The film prepared by the present invention is non-contractible; wherein, a large number of hydrogen bond network structures are formed between graphene oxide and polyacrylic acid macromolecular chains, and coordination bonds are formed between iron ions and graphene oxide and polyacrylic acid macromolecular chains, which can fix the structure of the film and make it water-resistant. The porous structure of graphene oxide gives the film a large specific surface area, and the non-contractibility prevents the specific surface area from being reduced. The non-contractibility and porous structure can expose more carboxyl groups to coordinate, load and fix a large number of iron ions in the film, so that the iron ion loading rate of the prepared film is higher and the iron ion leaching rate is low, and the large amount of stable presence of iron ions can make it have good catalytic activity.
[0025] Beneficial effects:
[0026] The invention discloses a method for preparing a non-shrinkable polyacrylic acid film. Formamide is introduced into a film-making solution and multivalent iron ions are introduced into a coagulation bath. The multivalent iron ions are used as a cross-linking agent and an active component of a catalytic reaction. On this basis, a small amount of graphene oxide is introduced as a modified material. The method is combined with a double stretching process and a heat setting process to promote the forming and stabilization of the non-shrinkable film and solve the problems of size shrinkage, poor mechanical properties, low iron ion loading and fixing ability of the polyacrylic acid film. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0028] The test method involved in the present invention is as follows:
[0029] (1) Tensile strength and elongation at break: used to characterize the mechanical properties of the film. The mechanical properties of the film samples were tested using a TSL electronic tensile testing machine (Jinan Sike Testing Technology Co., Ltd., China). The tensile speed was 10 cm / min, the temperature was 25 °C, the relative humidity was 30%, and the film clamp distance was 10 cm.
[0030] (2) Shrinkage rate: used to characterize the dimensional stability of the film; at 25°C, a certain length of film sample is immersed in 10 mL of deionized water. After soaking for 10 min, the length of the film after shrinkage is measured. The shrinkage rate of the film is calculated using the following formula:
[0031] ;
[0032] Where S is the shrinkage rate (%), Z0 is the length of the film before shrinkage (cm), and Z is the length of the film after shrinkage (cm).
[0033] (3) Dissolution rate: used to characterize the water resistance of the film; the film sample was placed in a filter paper bag and soaked in 85°C deionized water for 4 h. The filter paper bag was then taken out of the deionized water and placed in a 60°C vacuum drying oven for 12 h. The dried film sample was taken out of the filter paper bag and the dissolution rate of the film sample was calculated using the following formula:
[0034] ;
[0035] Wherein, G is the dissolution rate (%), m0 is the mass of the dry film before immersion and dissolution (g), m1 is the total mass of the film and the filter paper bag before immersion and dissolution (g), and m2 is the total mass of the film and the filter paper bag after drying (g).
[0036] (4) Specific surface area: The length, width and height of the film samples at five selected locations were measured multiple times and the average value was obtained. In addition, 20 films of the same specifications were accurately weighed and the specific surface area of the film was calculated according to the following formula based on the length, width and height of the film samples.
[0037] ;
[0038] Where K is the specific surface area of the film sample (m 2 / g); d is the length of the film sample (m); c is the width of the film sample (m); L is the height of the film sample (m); N is the mass of the film sample (g).
[0039] (5) Catalytic activity: At room temperature, add 10 mL of a 20 mg / L methylene blue aqueous solution into a 50 mL beaker. Use a pipette to measure 2 μL of H2O2 and add it to the beaker. Weigh 0.06 g of the film and place it in the methylene blue aqueous solution with H2O2. Shake the beaker continuously to obtain the target solution. Use a TU-1810 UV-visible spectrophotometer (Beijing Puxi General Instrument Co., Ltd., China) to monitor the absorbance of the target solution at a wavelength of 664 nm. Use the following formula to calculate the decolorization rate (DR) of the target solution to evaluate the catalytic performance of the film. When the DR is higher than 90%, remove the film sample from the beaker and use filter paper to remove the residual water on the surface of the film. Record the time required for the DR to reach 90% to obtain the catalytic activity. The decolorization rate (DR) is calculated as follows:
[0040] ;
[0041] Wherein, DR is the decolorization rate (%); C0 is the concentration of the initial methylene blue aqueous solution (mg / L); C1 is the concentration of the target solution (mg / L); C1 is obtained from the concentration-absorbance standard curve.
[0042] (6) Reusability: According to the above test steps for catalytic activity, the film was used again to decolorize a new methylene blue aqueous solution to evaluate its recyclability.
[0043] (7) Average iron ion leaching concentration: According to the steps described in the catalytic activity test, 0.06 g of the film was used to catalyze H2O2 to decolorize the methylene blue aqueous solution. When the decolorization rate reached the ideal value (i.e., above 90%), the film was separated from the methylene blue aqueous solution and the iron ion concentration in the methylene blue aqueous solution after decolorization was measured according to the method described in the literature (PEI / GO-codecorated poly(acrylic acid-co-hydroxyethylmethacrylate) fiber as a carrier to support iron ions and its catalytic performance for methylene blue decolorization[J]. Journal of Macromolecular Science Part A-Pure and Applied Chemistry, 2020, 57(7): 531-543.). During the process of recycling the film to decolorize the MB aqueous solution, the average iron ion leaching concentration was calculated. The calculation formula is:
[0044] mg / L;
[0045] Where, AE is the average iron ion leaching concentration (mg / L), A i is the absorbance value of the colorimetric solution after constant volume and calibration of the iron ion concentration, and n is the number of cycles.
[0046] (8) Iron ion loading rate: A certain mass of thin film samples was digested in an acidic environment with a pH of 2.5-4.0. The iron content in the solution after digestion was measured using an Agilent 5110 inductively coupled plasma optical emission spectrometer (ICP-OES) (Agilent, USA). The iron content in the thin film samples was quantified and the iron ion loading rate was calculated using the following formula.
[0047] ;
[0048] Where H is the iron ion loading rate (%); Q0 is the mass of the film sample (mg); Q1 is the iron content in the film sample (mg).
[0049] (9) Iron ion leaching rate: used to characterize the iron ion fixing ability of the film; according to the average iron ion leaching concentration test steps, the total mass of iron ions leached during the recycling of the film sample is calculated using formula (1), and then the iron element contained in the film sample is quantified according to the steps described in the iron ion loading rate. Finally, the iron ion leaching rate during the recycling of the film sample is calculated using formula (2).
[0050] (1);
[0051] (2);
[0052] In the formula, F m is the total mass of iron ions leached during the recycling of the film sample (mg); V i A is the volume of methylene blue aqueous solution when the membrane is used in each cycle (L); i is the absorbance value of the colorimetric solution calibrated with the iron ion concentration after constant volume; El is the iron ion leaching rate (%) during the recycling of the film sample; H is the iron ion loading rate (%); W is the mass of the film sample (mg).
[0053] The information of the raw material manufacturers used in the present invention is shown in Table 1:
[0054] Table 1
[0055]
[0056] Example 1
[0057] A method for preparing a non-shrinkable polyacrylic acid film, the specific steps are as follows:
[0058] (1) Acrylic acid and maleic anhydride with a mass ratio of 95:5 were subjected to free radical polymerization reaction under the action of benzoyl peroxide to obtain polyacrylic acid. The polymerization time was 2.5 h, the polymerization temperature was 85 °C, and the stirring speed during the polymerization was 180 r / min.
[0059] (2) adding graphene oxide to a mixed solvent consisting of water and formamide, magnetically stirring at room temperature for 30 min, and then ultrasonically dispersing for 30 min, then adding polyacrylic acid to the solution after ultrasonic dispersion, stirring at 85°C until completely dissolved, to prepare a membrane-forming solution, cooling to room temperature, and then standing the membrane-forming solution for 12 h to remove bubbles;
[0060] The mass ratio of polyacrylic acid, formamide and water in the membrane solution is 3.0:2.7:24.3, and the amount of graphene oxide added is 0.5 wt% of polyacrylic acid;
[0061] (3) After the film-forming solution is squeezed into a film using a film-forming device, the film is immersed in a coagulation bath for 4 hours, and then the film is taken out, stretched and heat-set in sequence to obtain a primary stretched film. Finally, the primary stretched film is immersed in a coagulation bath for 4 hours and then taken out, and then stretched and heat-set for a second time in sequence to obtain a non-shrinkable polyacrylic acid film.
[0062] Among them, the coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:4.12:11.78; the first stretching multiple is 20 times, and the first heat setting condition is: setting at a temperature of 60°C for 12 hours; the second stretching multiple is 1.4 times, and the second heat setting condition is: setting at a temperature of 60°C for 12 hours.
[0063] The specific surface area of the non-shrinkable polyacrylic acid film was 63.65×10 -3 m 2 / mg, tensile strength is 2.13cN / dtex, elongation at break is 34.59%, shrinkage after immersion in 25℃ water for 10min is 0, dissolution rate after immersion in 85℃ water for 4h is 25.17%, catalytic activity is 3min, iron ion loading rate at pH 3.5 is 11.29%, average iron ion leaching concentration is 2.24mg / L, iron ion leaching rate is 16.65%, and it can be reused 40 times.
[0064] Comparative Example 1
[0065] A method for preparing a polyacrylic acid film is basically the same as that of Example 1, except that the second stretching and heat setting operations in step (3) are omitted, that is, only one stretching and setting operation is performed.
[0066] The specific surface area of the polyacrylic acid film finally obtained is 42.17×10 -3 m 2 / mg, the tensile strength is 1.75cN / dtex, the elongation at break is 63.19%, the shrinkage rate after immersion in 25℃ water for 10min is 15.49%, the dissolution rate after immersion in 85℃ water for 4h is 34.16%, the iron ion loading rate at pH 3.5 is 7.48%, and the iron ion leaching rate is 23.64%.
[0067] By comparing Comparative Example 1 with Example 1, it can be found that compared with the film prepared under the secondary stretching and heat setting process, the film prepared under the single stretching and heat setting process has smaller specific surface area, tensile strength, and iron ion loading rate, while its elongation at break, shrinkage in water, solubility in water, and iron ion leaching rate are significantly larger. This is because compared with the secondary stretching and heat setting process, the film prepared under the single stretching and heat setting process has lower crystallization, orientation, and structural stability, so the performance of the film prepared under the single stretching and heat setting process is relatively poor.
[0068] Comparative Example 2
[0069] A method for preparing a polyacrylic acid film is basically the same as that in Example 1, except that: graphene oxide is not added in step (2), and the mass ratio of polyacrylic acid, formamide and water in the film-forming solution remains unchanged.
[0070] The specific surface area of the polyacrylic acid film finally obtained is 58.30×10 -3 m 2 / mg, the tensile strength is 1.86cN / dtex, the elongation at break is 43.75%, the shrinkage rate after immersion in 25℃ water for 10min is 13.21%, the dissolution rate after immersion in 85℃ water for 4h is 28.76%, the iron ion loading rate at pH 3.5 is 5.73%, and the iron ion leaching rate is 61.76%.
[0071] By comparing Comparative Example 2 with Example 1, it can be found that compared with the film prepared by adding graphene oxide, the film prepared without adding graphene oxide has smaller specific surface area, tensile strength, and iron ion loading rate, while its elongation at break, shrinkage in water, solubility in water, and iron ion leaching rate are larger. This is because graphene oxide can strengthen the interaction between polyacrylic acid macromolecular chains, effectively control the movement of polyacrylic acid macromolecular chains and strengthen the internal structure of the film, making it non-shrinkable, and the stable hydrogen bond network and ion cross-linking network (the hydroxyl and carboxyl groups contained in graphene oxide can coordinate and cross-link with iron ions to form an ion cross-linking network) are helpful for the film to load and fix iron ions, so the performance of the film prepared without adding graphene oxide is relatively poor.
[0072] Comparative Example 3
[0073] A method for preparing a polyacrylic acid film is basically the same as that in Example 1, except that the amount of graphene oxide added in step (2) is 0.2 wt %.
[0074] The specific surface area of the polyacrylic acid film finally obtained is 54.41×10 -3 m 2 / mg, the tensile strength is 1.94cN / dtex, the elongation at break is 40.67%, the shrinkage after immersion in 25℃ water for 10min is 11.69%, the dissolution rate after immersion in 85℃ water for 4h is 26.84%, the iron ion loading rate is 6.34%, and the iron ion leaching rate is 52.18%.
[0075] By comparing Comparative Example 3 with Example 1, it can be found that the addition of a lower content of graphene oxide does not significantly improve the various properties of the film. This is because the addition of a low content of graphene oxide is not sufficient to strengthen the interaction between the polyacrylic acid macromolecular chains, so the prepared film cannot obtain a stable structure and good performance.
[0076] Comparative Example 4
[0077] A method for preparing a polyacrylic acid film is basically the same as that in Example 1, except that the amount of graphene oxide added in step (2) is 2.1 wt %.
[0078] The specific surface area of the polyacrylic acid film finally obtained is 49.68×10 -3 m 2 / mg, the tensile strength is 1.89cN / dtex, the elongation at break is 38.47%, the shrinkage rate after immersion in 25℃ water for 10min is 4.76%, the dissolution rate after immersion in 85℃ water for 4h is 25.48%, the iron ion loading rate at pH 3.5 is 9.87%, and the iron ion leaching rate is 26.49%.
[0079] By comparing Comparative Example 4 with Example 1, it can be found that the addition of excessive graphene oxide will cause the various properties of the film to deteriorate. This is because the addition of excessive graphene oxide will cause uneven dispersion and agglomeration of graphene oxide in the film, and the prepared film has more structural defects, poor structural stability, reduced specific surface area, tensile strength and water resistance, and its loading and fixing ability for iron ions deteriorate. Therefore, the addition of excessive graphene oxide will cause the various properties of the film to deteriorate.
[0080] Comparative Example 5
[0081] A method for preparing a polyacrylic acid film is basically the same as that of Example 1, except that the coagulation bath in step (3) does not contain ferric chloride.
[0082] The specific surface area of the polyacrylic acid film finally obtained is 42.89×10 -3 m 2 / mg, the tensile strength is 1.42cN / dtex, the elongation at break is 84.16%, the shrinkage rate after immersion in 25℃ water for 10min is 27.81%, the dissolution rate after immersion in 85℃ water for 4h is 31.71%, the iron ion loading rate at pH 3.5 is 5.38%, and the iron ion leaching rate is 64.97%.
[0083] By comparing Comparative Example 5 with Example 1, it can be found that the absence of ferric chloride in the coagulation bath is not conducive to the improvement of various properties of the film. This is because Fe 2+ It will form a loose and changeable coordination cross-linking network with the polyacrylic acid macromolecular chain, which will cause the prepared film matrix to be too fluffy and the internal cross-linking structure to be loose. Although graphene oxide will form a hydrogen bond network with the polyacrylic acid macromolecular chain, it is not enough to stabilize its structure and prevent size shrinkage. In addition, its ability to fix iron ions is insufficient. Therefore, the performance of the film prepared without ferric chloride in the coagulation bath is poor.
[0084] Comparative Example 6
[0085] A method for preparing a polyacrylic acid film is basically the same as that of Example 1, except that the coagulation bath in step (3) does not contain ferrous chloride.
[0086] The specific surface area of the polyacrylic acid film finally obtained is 32.16×10 -3 m 2 / mg, the tensile strength is 1.63cN / dtex, the elongation at break is 31.16%, the shrinkage after immersion in 25℃ water for 10min is 22.17%, and the iron ion loading rate at pH 3.5 is 7.16%.
[0087] By comparing Comparative Example 6 with Example 1, it can be found that the absence of ferrous chloride in the coagulation bath will also cause the performance of the film to deteriorate. This is because Fe 3+ It will form a dense and stable coordination cross-linking network with the polyacrylic acid macromolecular chain, and the film has not completely relaxed the internal stress existing in the matrix during the stretching and heat setting process. Some internal stress will still remain in the prepared film, which is not conducive to the stretching and dimensional stability of the film, thereby resulting in a reduction in the film stretching multiple, and the film matrix is easy to break and brittle, its specific surface area and tensile strength are greatly reduced, and the shrinkage rate in water is increased. Due to the significant reduction in specific surface area, its iron ion loading rate is reduced.
[0088] Comparative Example 7
[0089] A method for preparing a polyacrylic acid film is basically the same as that of Example 1, except that the coagulation bath in step (3) does not contain ferric chloride and ferrous chloride.
[0090] The specific surface area of the polyacrylic acid film finally obtained is 27.63×10 -3 m 2 / mg, the tensile strength is 0.74cN / dtex, the elongation at break is 58.46%, the shrinkage rate after immersion in 25℃ water for 10min is 38.49%, the dissolution rate after immersion in 85℃ water for 4h is 34.79%, the iron ion loading rate at pH 3.5 is 3.46%, and the iron ion leaching rate is 72.64%.
[0091] By comparing Comparative Example 7 with Example 1, it can be found that the absence of iron ions in the coagulation bath will lead to a significant decrease in the performance of the film. This is because it is impossible to obtain a film with a stable structure and excellent performance by relying solely on the interaction between the polyacrylic acid macromolecular chains without the coordination and cross-linking effect between the iron ions and the polyacrylic acid macromolecular chains. Therefore, the performance of the film prepared without the presence of iron ions in the coagulation bath is relatively poor.
[0092] Example 2
[0093] A method for preparing a non-shrinkable polyacrylic acid film, the specific steps are as follows:
[0094] (1) Acrylic acid and maleic anhydride with a mass ratio of 95:5 were subjected to free radical polymerization reaction under the action of benzoyl peroxide to obtain polyacrylic acid. The polymerization time was 2.5 h, the polymerization temperature was 85 °C, and the stirring speed during the polymerization was 180 r / min.
[0095] (2) adding graphene oxide to a mixed solvent consisting of water and formamide, magnetically stirring at room temperature for 30 min, and then ultrasonically dispersing for 30 min, then adding polyacrylic acid to the solution after ultrasonic dispersion, stirring at 85°C until completely dissolved, to prepare a membrane-forming solution, cooling to room temperature, and then standing the membrane-forming solution for 12 h to remove bubbles;
[0096] The mass ratio of polyacrylic acid, formamide and water in the membrane solution is 3.0:5.4:21.6, and the amount of graphene oxide added is 0.5 wt% of polyacrylic acid;
[0097] (3) After the film-forming solution is squeezed into a film using a film-forming device, the film is immersed in a coagulation bath for 4 hours, and then the film is taken out, stretched and heat-set in sequence to obtain a primary stretched film. Finally, the primary stretched film is immersed in a coagulation bath for 4 hours and then taken out, and then stretched and heat-set for a second time in sequence to obtain a non-shrinkable polyacrylic acid film.
[0098] Among them, the coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:4.12:11.78; the first stretching multiple is 19 times, and the first heat setting condition is: setting at a temperature of 80°C for 10 hours; the second stretching multiple is 1.45 times, and the second heat setting condition is: setting at a temperature of 80°C for 10 hours.
[0099] The specific surface area of the non-shrinkable polyacrylic acid film was 59.87×10 -3 m 2 / mg, tensile strength is 1.95cN / dtex, elongation at break is 39.42%, shrinkage after immersion in 25℃ water for 10min is 0, dissolution rate after immersion in 85℃ water for 4h is 26.79%, catalytic activity is 4min, iron ion loading rate at pH 3.5 is 10.34%, average iron ion leaching concentration is 2.46mg / L, iron ion leaching rate is 19.64%, and it can be reused 40 times.
[0100] Example 3
[0101] A method for preparing a non-shrinkable polyacrylic acid film, the specific steps are as follows:
[0102] (1) Acrylic acid and maleic anhydride with a mass ratio of 95:5 were subjected to free radical polymerization reaction under the action of benzoyl peroxide to obtain polyacrylic acid. The polymerization time was 2.5 h, the polymerization temperature was 85 °C, and the stirring speed during the polymerization was 180 r / min.
[0103] (2) adding graphene oxide to a mixed solvent consisting of water and formamide, magnetically stirring at room temperature for 30 min, and then ultrasonically dispersing for 30 min, then adding polyacrylic acid to the solution after ultrasonic dispersion, stirring at 85°C until completely dissolved, to prepare a membrane-forming solution, cooling to room temperature, and then standing the membrane-forming solution for 12 h to remove bubbles;
[0104] The mass ratio of polyacrylic acid, formamide and water in the membrane solution is 3.0:10.8:16.2, and the amount of graphene oxide added is 0.25 wt% of polyacrylic acid;
[0105] (3) After the film-forming solution is squeezed into a film using a film-forming device, the film is immersed in a coagulation bath for 4 hours, and then the film is taken out, stretched and heat-set in sequence to obtain a primary stretched film. Finally, the primary stretched film is immersed in a coagulation bath for 4 hours and then taken out, and then stretched and heat-set for a second time in sequence to obtain a non-shrinkable polyacrylic acid film.
[0106] Among them, the coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:4.12:11.78; the first stretching multiple is 20 times, and the first heat setting condition is: setting at a temperature of 100°C for 5 hours; the second stretching multiple is 1.5 times, and the second heat setting condition is: setting at a temperature of 100°C for 5 hours.
[0107] The specific surface area of the non-shrinkable polyacrylic acid film was 69.87×10 -3 m 2 / mg, tensile strength is 1.87cN / dtex, elongation at break is 46.58%, shrinkage after immersion in 25℃ water for 10min is 0, dissolution rate after immersion in 85℃ water for 4h is 27.68%, catalytic activity is 5min, iron ion loading rate at pH 3.5 is 9.46%, average iron ion leaching concentration is 2.57mg / L, iron ion leaching rate is 13.67%, and it can be reused 40 times.
[0108] Example 4
[0109] A method for preparing a non-shrinkable polyacrylic acid film, the specific steps are as follows:
[0110] (1) Acrylic acid and maleic anhydride with a mass ratio of 95:5 were subjected to free radical polymerization reaction under the action of benzoyl peroxide to obtain polyacrylic acid. The polymerization time was 2.5 h, the polymerization temperature was 85 °C, and the stirring speed during the polymerization was 180 r / min.
[0111] (2) adding graphene oxide to a mixed solvent consisting of water and formamide, magnetically stirring at room temperature for 30 min, and then ultrasonically dispersing for 30 min, then adding polyacrylic acid to the solution after ultrasonic dispersion, stirring at 85°C until completely dissolved, to prepare a membrane-forming solution, cooling to room temperature, and then standing the membrane-forming solution for 12 h to remove bubbles;
[0112] The mass ratio of polyacrylic acid, formamide and water in the membrane solution is 3.0:8.1:18.9, and the amount of graphene oxide added is 1.0wt% of polyacrylic acid;
[0113] (3) After the film-forming solution is squeezed into a film using a film-forming device, the film is immersed in a coagulation bath for 4 hours, and then the film is taken out, stretched and heat-set in sequence to obtain a primary stretched film. Finally, the primary stretched film is immersed in a coagulation bath for 4 hours and then taken out, and then stretched and heat-set for a second time in sequence to obtain a non-shrinkable polyacrylic acid film.
[0114] Among them, the coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:5.49:10.10; the first stretching multiple is 17 times, and the first heat setting condition is: setting at a temperature of 120°C for 1 hour; the second stretching multiple is 1.45 times, and the second heat setting condition is: setting at a temperature of 120°C for 2.5 hours.
[0115] The specific surface area of the non-shrinkable polyacrylic acid film was 54.81×10 -3 m 2 / mg, tensile strength is 1.81cN / dtex, elongation at break is 54.67%, shrinkage after immersion in 25℃ water for 10min is 0, dissolution rate after immersion in 85℃ water for 4h is 27.28%, catalytic activity is 6min, iron ion loading rate at pH 3.5 is 8.65%, average iron ion leaching concentration is 4.58mg / L, iron ion leaching rate is 32.46%, and it can be reused 40 times.
[0116] Example 5
[0117] A method for preparing a non-shrinkable polyacrylic acid film, the specific steps are as follows:
[0118] (1) Acrylic acid and maleic anhydride with a mass ratio of 95:5 were subjected to free radical polymerization reaction under the action of benzoyl peroxide to obtain polyacrylic acid. The polymerization time was 2.5 h, the polymerization temperature was 85 °C, and the stirring speed during the polymerization was 180 r / min.
[0119] (2) adding graphene oxide to a mixed solvent consisting of water and formamide, magnetically stirring at room temperature for 30 min, and then ultrasonically dispersing for 30 min, then adding polyacrylic acid to the solution after ultrasonic dispersion, stirring at 85°C until completely dissolved, to prepare a membrane-forming solution, cooling to room temperature, and then standing the membrane-forming solution for 12 h to remove bubbles;
[0120] The mass ratio of polyacrylic acid, formamide and water in the membrane solution is 3.0:2.7:24.3, and the amount of graphene oxide added is 2.0wt% of polyacrylic acid;
[0121] (3) After the film-forming solution is squeezed into a film using a film-forming device, the film is immersed in a coagulation bath for 4 hours, and then the film is taken out, stretched and heat-set in sequence to obtain a primary stretched film. Finally, the primary stretched film is immersed in a coagulation bath for 4 hours and then taken out, and then stretched and heat-set for a second time in sequence to obtain a non-shrinkable polyacrylic acid film.
[0122] Among them, the coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:5.49:10.10; the first stretching multiple is 16 times, and the first heat setting condition is: setting at a temperature of 140°C for 0.5h; the second stretching multiple is 1.4 times, and the second heat setting condition is: setting at a temperature of 140°C for 0.5h.
[0123] The specific surface area of the non-shrinkable polyacrylic acid film was 51.49×10 -3 m 2 / mg, tensile strength is 1.78cN / dtex, elongation at break is 61.23%, shrinkage after immersion in 25℃ water for 10min is 0, dissolution rate after immersion in 85℃ water for 4h is 21.48%, catalytic activity is 7min, iron ion loading rate at pH 3.5 is 8.47%, average iron ion leaching concentration is 5.49mg / L, iron ion leaching rate is 69.78%, and it can be reused 40 times.
Claims
1. A method for preparing a non-shrinkable polyacrylic acid film, characterized in that: After the film-forming solution is squeezed into a film by a film-forming device, the film is immersed in a coagulation bath, and then the film is taken out, stretched and heat-set in sequence to obtain a primary stretched film, and finally the primary stretched film is immersed in a coagulation bath, taken out, stretched and heat-set in sequence to obtain a non-shrinkable polyacrylic acid film; The membrane-forming solution is composed of polyacrylic acid, formamide, water and graphene oxide, and the added amount of graphene oxide is 0.25-2.0wt% of the polyacrylic acid, and the mass ratio of polyacrylic acid, formamide and water in the membrane-forming solution is 3.0:2.7-10.8:16.2-24.3; The polyacrylic acid is obtained by free radical polymerization of acrylic acid and maleic anhydride in a mass ratio of 95:5 under the action of benzoyl peroxide, the polymerization time is 2.5 hours, the polymerization temperature is 85° C., and the stirring speed during the polymerization is 180 r / min; The coagulation bath is a mixture of concentrated sulfuric acid, water, ferric chloride and ferrous chloride in a mass ratio of 30:100:4.12~5.49:10.10~11.78; The first stretching multiple is 16-20 times, and the first heat setting condition is: setting at 60-140℃ for 0.5-12h; The second stretching multiple is 1.4~1.5 times, and the second heat setting condition is: setting at 60~140℃ for 0.5~12h; The shrinkage rate of the non-shrinkable polyacrylic acid film when immersed in water at 25° C. for 10 minutes is 0.
2. The method for preparing a non-shrinkable polyacrylic acid film according to claim 1, characterized in that: The specific surface area of the non-shrinkable polyacrylic acid film is 51.49×10 -3 ~69.87×10 -3 m 2 / mg, the dissolution rate after immersion in 85℃ water for 4h was 21.48~27.68%, the catalytic activity was 3~7min, the iron ion loading rate was 8.47~11.29%, and the iron ion leaching rate was 13.67~69.78%.
3. The method for preparing a non-shrinkable polyacrylic acid film according to claim 1, characterized in that: The first immersion treatment in the coagulation bath lasts for 4 hours.
4. The method for preparing a non-shrinkable polyacrylic acid film according to claim 3, characterized in that: The second immersion treatment time in the coagulation bath is 4 hours.
Citation Information
Patent Citations
Preparation method of graphene oxide-polyacrylic acid mother of pearl imitated laminar composite film
CN109504012A
Method for preparing composite polymer electrolyte thin film by doping
CN105244537A
Ultrathin shrinkage-resistant high-liquid-absorption and high-liquid-retention lithium battery diaphragm and preparation method thereof
CN117712621A
process for manufacturing a non-heat-shrinkable transparent polyamide film and product obtained thereby
FR1542176A
Microporous polyolefin membrane and method for producing the same
US20090098341A1