A platinum metal complex supported on an organosolid salt containing a sulfoxide functional group for catalyzing hydrosilylation reactions and its synthesis method.
By using a platinum metal complex catalyst supported on 3-(methylsulfinyl)propionate, the problem of insufficient stability of homogeneous catalysts was solved, realizing a highly efficient and pollution-free hydrosilylation reaction. The catalyst has high activity and is easy to recover, making it suitable for industrial production.
Patent Information
- Application Number
- CN202410378273.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing homogeneous platinum catalysts are not stable enough in hydrosilylation reactions, are difficult to recycle, and are prone to generating platinum black, resulting in low reaction efficiency and product contamination.
A platinum metal complex catalyst was prepared by supporting a platinum metal complex catalyst with 3-(methylsulfinyl)propionate and reacting under an inert atmosphere to form a heterogeneous catalyst, thereby avoiding the formation of platinum black and improving recyclability.
It improves the yield and selectivity of hydrosilylation reaction, has good catalyst stability, produces no platinum black after reaction, is easy to recycle and reuse, and is suitable for industrial applications.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0004767650470000011
Abstract
Description
Technical Field
[0001] This invention relates to the field of fine chemicals, specifically to a novel organic solid salt-supported platinum metal complex containing sulfoxide functional groups and its synthesis method, for use in catalyzing hydrosilylation reactions. Background Technology
[0002] Hydrosilylation reactions refer to the addition reactions between organic or inorganic silicon-hydrogen bonds and unsaturated bonds. Among these, the reactions with carbon-carbon double and triple bonds are the most widely studied. Furthermore, because hydrosilylation is the simplest and most economical method for obtaining organosilicon, and with the increasing demand for silicon products, it has become a hot topic for exploration and innovation in related fields. Hydrosilylation reactions are usually catalyzed by transition metals and their complexes, such as Pt, Pd, Rh, Ru, Ni, and their complexes. Pt metal complex catalysts are the most widely used, with Speier and Karstedt catalysts being the most typical. While these catalysts exhibit high catalytic activity, as homogeneous catalysts, they suffer from insufficient stability, are prone to platinum black formation, and are difficult to recover and reuse after the reaction.
[0003] Supported catalysts are composite catalysts formed by loading one catalyst onto another material, resulting in higher efficiency. Common inorganic material supports include alumina, silica, calcium carbonate, and activated carbon, which offer advantages such as good thermal stability and low cost. However, they also suffer from insufficient nucleophilicity, making it difficult to form stable chemical bonds with positively charged Pt, thus hindering the maintenance of Pt catalyst loading and preventing platinum black formation during reactions. Therefore, researching and preparing novel supported catalysts with high reactivity, high selectivity, and easy recovery is of significant value for industrial applications. Summary of the Invention
[0004] To address the problems of existing technologies, this invention provides a novel solid salt-supported platinum metal complex catalyst and its synthesis method. The catalyst is synthesized under mild conditions, is easy to separate and recover, and can improve the yield and selectivity of hydrosilylation reactions.
[0005] The objective of this invention is achieved through the following technical solution:
[0006] This invention provides a catalyst for catalyzing hydrosilylation reactions, wherein the catalyst uses 3-(methylsulfinyl)propionate as a support and supports a platinum metal complex catalyst; the structural formula of the 3-(methylsulfinyl)propionate is:
[0007]
[0008] Furthermore, in the above technical solution, the platinum metal complex catalyst is a platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex.
[0009] Furthermore, in the above technical solution, the molar ratio of 3-(methylsulfinyl)propionate and platinum metal complex catalyst is 1:0.5-1.5; preferably 1:1.
[0010] Furthermore, in the above technical solution, the preparation method of 3-(methylsulfinyl)propionate includes: diluting 3-methylthiopropionic acid and adding 30% hydrogen peroxide, stirring at room temperature, and removing the solvent to obtain 3-(methylsulfinyl)propionic acid;
[0011] Calcium 3-(methylsulfinyl)propionic acid is prepared by reacting it with calcium hydroxide or barium hydroxide, filtering, and collecting the precipitate.
[0012] Furthermore, in the above technical solution, the preparation method of the catalyst includes: mixing and stirring 3-(methylsulfinyl)propionate with a platinum metal complex catalyst, the preparation route being as follows:
[0013]
[0014] Furthermore, in the above technical solution, the method for preparing the catalyst uses an inert gas atmosphere, toluene as the solvent for the reaction, a reaction temperature of 20-30℃, and a reaction time of 2-10h.
[0015] The present invention also provides the application of the aforementioned catalyst in catalytic hydrosilylation reactions.
[0016] Furthermore, in the above technical solution, the reaction involves reacting an unsaturated product containing carbon-carbon double or triple bonds with a silane reagent. The unsaturated product is allyl glycidyl ether, 1-octene, 2-methyl-3-butyn-2-ol, or styrene. The silane reagent is trimethoxysilane. The molar ratio of the unsaturated product to trimethoxysilane is 1:1-1.5, preferably 1:1.2.
[0017] Furthermore, in the above technical solution, the reaction temperature of the catalytic hydrosilylation reaction is 60-80℃; the reaction time is 8-12h; the reaction solvent is a hydrocarbon solvent, preferably toluene; and the reaction atmosphere is an inert gas, preferably nitrogen.
[0018] Furthermore, in the above technical solution, the reaction formula between allyl glycidyl ether and trimethoxysilane is as follows:
[0019]
[0020] Furthermore, in the above technical solution, the reaction formula between 1-octene and trimethoxysilane is as follows:
[0021]
[0022] Furthermore, in the above technical solution, the reaction formula between 2-methyl-3-butyn-2-ol and trimethoxysilane is as follows:
[0023]
[0024] Furthermore, in the above technical solution, the reaction formula between styrene and trimethoxysilane is as follows:
[0025]
[0026] The beneficial effects of this invention are:
[0027] (1) The present invention prepares a novel solid salt supported platinum metal complex catalyst. This catalyst is a heterogeneous catalyst in the reaction system. Generally speaking, its specific surface area and contact rate are smaller than those of homogeneous catalysts. However, in the catalytic hydrosilylation reaction, the yield and selectivity obtained by this catalyst are greater than those of the unsupported platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex. This indicates that the catalyst has high activity. At the same time, the support is stable and readily available, and easy to recover, making it more suitable for the industrialization of hydrosilylation.
[0028] (2) The catalyst prepared by the present invention is supported by organic salt. When the catalyst is applied to the hydrosilylation reaction, no platinum black is generated, the product is not contaminated, and it can be recycled and reused.
[0029] (3) When the catalyst prepared in this invention is applied to the silane-hydrogen reaction of unsaturated hydrocarbon compounds, such as in the silane-hydrogen reaction of 2-methyl-3-butyn-2-ol with trimethoxysilane, the reaction yield can reach 100.0%. Attached Figure Description
[0030] Figure 1 : Gas phase spectrum of the hydrosilylation reaction of allyl glycidyl ether catalyzed in Example 3.
[0031] Figure 2 : Gas phase spectrum of the hydrosilylation reaction of allyl glycidyl ether catalyzed in Example 4.
[0032] Figure 3 : Gas phase spectrum of the catalytic addition reaction of 1-octene in Example 5.
[0033] Figure 4 : Gas phase spectrum of the catalytic addition reaction of 1-octene in Example 6.
[0034] Figure 5Gas phase spectrum of the catalytic addition reaction of 2-methyl-3-butyn-2-ol in Example 7.
[0035] Figure 6 : Gas phase spectrum of the catalytic addition reaction of 2-methyl-3-butyn-2-ol in Example 8.
[0036] Figure 7 Gas phase spectrum of the catalytic styrene addition reaction in Example 9.
[0037] Figure 8 : Gas phase spectrum of the catalytic styrene addition reaction in Example 10.
[0038] Figure 9 NMR spectrum of 3-(methylsulfinyl)propionic acid.
[0039] Figure 10 Infrared spectrum of 3-(methylsulfinyl)propionate. Detailed Implementation
[0040] The following non-limiting embodiments are intended to enable those skilled in the art to more fully understand the present invention, but do not limit the invention in any way.
[0041] Unless otherwise specified, the experimental methods described in the following examples are conventional methods; the reagents and materials described are commercially available unless otherwise specified.
[0042] The preparation method of 3-(methylsulfinyl)propionate is as follows: 498 mg (4.144 mmol) of 3-methylthiopropionic acid was added to a 25 mL three-necked flask, diluted with 2 mL of distilled water, and then 0.5 mL of 30% hydrogen peroxide was added. The solution was stirred at room temperature for 48 hours, and then the solvent water was removed to obtain almost pure 3-(methylsulfinyl)propionic acid. Figure 9 It can be seen that, 1 ¹H NMR (400MHz, CD₃OD₃SPE) δ 3.15 (dt, J = 13.4, 7.7 Hz, 1H), 2.97 (dt, J = 13.4, 6.7 Hz, 1H), 2.74 (t, J = 7.3 Hz, 2H), 2.66 (s, 3H); 3-(methylsulfinyl)propionic acid with the chemical formula C₄H₈O₃S was prepared.
[0043] Calcium 3-(methylsulfinyl)propionic acid is prepared by reacting it with calcium hydroxide, filtering, and collecting the precipitate. Similarly, barium 3-(methylsulfinyl)propionic acid is prepared by reacting it with barium hydroxide, filtering, and collecting the precipitate. Figure 10 A more noticeable peak appears at 1070cm -1 1460cm -11750cm -1 Nearby; 1070cm -1 The nearby peak is caused by the stretching vibration of S=O, 1750cm -1 The nearby peak is caused by the stretching vibration of C=O, 1460 cm⁻¹ -1 The nearby peak is caused by the deformation vibration of CH2, 3430 cm⁻¹ -1 The broad peak at the point is caused by the OH bond in H2O; it can be seen that calcium 3-(methylsulfinyl)propionate and barium 3-(methylsulfinyl)propionate were prepared.
[0044] Example 1: Synthesis of calcium salt supported platinum metal complex catalyst
[0045] Weigh 8 mg (0.026 mmol) of calcium 3-(methylsulfinyl)propionate and add it to a 50 mL three-necked flask. Then add 10 mg (0.026 mmol) of platinum(0)-1,3-diethylene-1,1,3,3-tetraglyceride methyldisiloxane complex (Karstedt catalyst). Use 3 mL of toluene as solvent, under N2 protection, stir at 25 °C for 10 h. The reaction was complete by TLC, and the calcium salt supported platinum metal complex catalyst was obtained.
[0046] Example 2: Synthesis of Barium Salt-Supported Platinum Metal Complex Catalyst
[0047] Weigh 10 mg (0.026 mmol) of barium 3-(methylsulfinyl)propionate and add it to a 50 mL three-necked flask. Then add 10 mg (0.026 mmol) of platinum(O)-1,3-diethylene-1,1,3,3-tetraglyceride methyldisiloxane complex (Karstedt catalyst). Use 3 mL of toluene as solvent, under N2 protection, stir at 25 °C for 10 h. The Karstedt catalyst was completely reacted by TLC, and the barium salt supported platinum metal complex catalyst was obtained.
[0048] Comparative Example 1: Hydrosilylation of allyl glycidyl ethers catalyzed by platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex.
[0049] 642 mg (5.257 mmol) of trimethoxysilane and 500 mg (4.381 mmol) of allyl glycidyl ether were added to a 50 mL three-necked flask. Under N2 protection, 10 mg of Karstedt catalyst (platinum(O)-1,3-diethylene-1,1,3,3-tetraglyceride methyldisiloxane complex) and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 66.4% according to the gas phase spectrum.
[0050] Example 3: Hydrosilylation reaction of allyl glycidyl ether catalyzed by a calcium salt-supported platinum metal complex catalyst
[0051] In this embodiment, except that 10 mg of platinum(0)-1,3-diethylene-1,1,3,3-tetraglyceride methyldisiloxane complex was replaced with the calcium salt supported platinum metal complex catalyst prepared in Example 1, the other conditions and steps were the same as in Comparative Example 1. The yield was approximately 87.5% based on the gas phase chromatogram.
[0052] As can be seen from Example 3 and Comparative Example 1, the catalyst proposed significantly improves the yield in the hydrosilylation reaction of allyl glycidyl ether, increasing the yield from 66.4% to 87.5%. Furthermore, no platinum black was observed in the reaction solution during the reaction process in Example 3.
[0053] Example 4: Hydrosilylation reaction of allyl glycerol ethers catalyzed by a barium salt-supported platinum metal complex catalyst.
[0054] In this embodiment, except that 10 mg of platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex was replaced with the barium salt-supported platinum metal complex catalyst prepared in Example 2, the other conditions and steps were the same as in Comparative Example 1. The yield was approximately 87.3% based on the gas phase chromatogram.
[0055] As can be seen from Example 4 and Comparative Example 1, the catalyst of this application significantly improves the yield in the hydrosilylation reaction of allyl glycidyl ether, increasing the yield from 66.4% to 87.3%.
[0056] Comparative Example 2: Hydrosilylation of 1-octene catalyzed by platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex
[0057] 642 mg (5.257 mmol) of trimethoxysilane and 491 mg (4.381 mmol) of 1-octene were added to a 50 mL three-necked flask. Under N2 protection, 10 mg of Karstedt catalyst and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 58.5% based on the gas phase chromatogram.
[0058] Example 5: Hydrosilylation of 1-octene catalyzed by a calcium salt-supported platinum metal complex catalyst
[0059] 642 mg (5.257 mmol) of trimethoxysilane and 491 mg (4.381 mmol) of 1-octene were added to a 50 mL three-necked flask. Under N2 protection, the calcium salt-supported platinum metal complex catalyst prepared in Example 1 and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 61.6% according to the gas phase chromatogram.
[0060] Example 6: Hydrosilylation of 1-octene catalyzed by a barium salt-supported platinum metal complex catalyst
[0061] 642 mg (5.257 mmol) of trimethoxysilane and 491 mg (4.381 mmol) of 1-octene were added to a 50 mL three-necked flask. Under N2 protection, the barium salt-supported platinum metal complex catalyst prepared in Example 2 and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 66.5% according to the gas phase chromatogram.
[0062] As can be seen from Examples 5, 6 and Comparative Example 2, the catalyst of this application significantly improves the yield in the hydrosilylation reaction of 1-octene.
[0063] Comparative Example 3: Hydrosilylation of 2-methyl-3-butyn-2-ol catalyzed by platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex
[0064] 642 mg (5.257 mmol) of trimethoxysilane and 368 mg (4.381 mmol) of 2-methyl-3-butyn-2-ol were added to a 50 mL three-necked flask. Under N2 protection, 10 mg of Karstedt catalyst and 15 mL of toluene were added. The reaction was maintained at 80 °C for 10 h. The yield was approximately 78.9% based on the gas phase chromatogram.
[0065] Example 7: Hydrosilylation of 2-methyl-3-butyn-2-ol catalyzed by a calcium salt-supported platinum metal complex catalyst
[0066] 642 mg (5.257 mmol) of trimethoxysilane and 368 mg (4.381 mmol) of 2-methyl-3-butyn-2-ol were added to a 50 mL three-necked flask. Under N2 protection, the calcium salt-supported platinum metal complex catalyst prepared in Example 1 and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 100.0% according to the gas phase chromatogram.
[0067] Example 8: Hydrosilylation of 2-methyl-3-butyn-2-ol catalyzed by a barium salt-supported platinum metal complex catalyst
[0068] 642 mg (5.257 mmol) of trimethoxysilane and 368 mg (4.381 mmol) of 2-methyl-3-butyn-2-ol were added to a 50 mL three-necked flask. Under N2 protection, the barium salt-supported platinum metal complex catalyst prepared in Example 2 and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 100.0% according to the gas phase chromatogram.
[0069] As can be seen from Examples 7, 8 and Comparative Example 3, the catalyst of this application significantly improves the yield in the hydrosilylation reaction of 2-methyl-3-butyn-2-ol, with the yield reaching 100%.
[0070] Comparative Example 4: Hydrosilylation of Styrene Catalyzed by Platinum(O)-1,3-Diethylene-1,1,3,3-Tetramethyldisiloxane Complex
[0071] 642 mg (5.257 mmol) of trimethoxysilane and 456 mg (4.381 mmol) of styrene were added to a 50 mL three-necked flask. Under N2 protection, 10 mg of Karstedt catalyst and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 53.2% based on the gas phase chromatogram.
[0072] Example 9: Hydrosilylation of styrene catalyzed by calcium salt-supported platinum metal complex catalyst
[0073] 642 mg (5.257 mmol) of trimethoxysilane and 456 mg (4.381 mmol) of styrene were added to a 50 mL three-necked flask. Under N2 protection, the calcium salt-supported platinum metal complex catalyst prepared in Example 1 and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 60.7% according to the gas phase chromatogram.
[0074] Example 10: Hydrosilylation of styrene catalyzed by barium salt-supported platinum metal complex catalyst
[0075] 642 mg (5.257 mmol) of trimethoxysilane and 456 mg (4.381 mmol) of styrene were added to a 50 mL three-necked flask. Under N2 protection, the barium salt-supported platinum metal complex catalyst prepared in Example 2 and 15 mL of toluene were added. The reaction temperature was controlled at 80 °C, and the reaction time was 10 h. The yield was approximately 62% according to the gas phase chromatogram.
[0076] As can be seen from Examples 9, 10 and Comparative Example 4, the catalyst of this application significantly improves the yield in the hydrosilylation reaction of styrene.
[0077] For anyone skilled in the art, many possible variations and modifications can be made to the technical solutions of this invention, or equivalent embodiments can be modified based on the disclosed technical content, without departing from the scope of the technical solutions of this invention. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of this invention without departing from the content of the technical solutions of this invention should still fall within the protection scope of the technical solutions of this invention.
Claims
1. A catalyst for catalyzing hydrosilylation reactions, characterized in that, The catalyst uses 3-(methylsulfinyl)propionate as a support and supports a platinum metal complex catalyst; the structural formula of the 3-(methylsulfinyl)propionate is: The platinum metal complex catalyst is a platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex; the molar ratio of 3-(methylsulfinyl)propionate to the platinum metal complex catalyst is 1:0.5-1.
5.
2. The catalyst according to claim 1, characterized in that, The preparation method of the 3-(methylsulfinyl)propionate includes: diluting 3-methylthiopropionic acid and adding 30% hydrogen peroxide, stirring at room temperature, and removing the solvent to obtain 3-(methylsulfinyl)propionic acid; Calcium 3-(methylsulfinyl)propionic acid is prepared by reacting it with calcium hydroxide or barium hydroxide, filtering, and collecting the precipitate.
3. The catalyst according to claim 1, characterized in that, The catalyst is prepared by mixing and stirring 3-(methylsulfinyl)propionate with a platinum metal complex catalyst, and the preparation route is as follows: 。 4. The catalyst according to claim 3, characterized in that, The preparation method uses an inert gas atmosphere, toluene as the solvent, a reaction temperature of 20-30℃, and a reaction time of 2-10h.
5. The application of the catalyst according to any one of claims 1 to 4 in the catalytic hydrosilylation reaction.
6. The application according to claim 5, wherein the reaction is carried out with an unsaturated product containing a carbon-carbon double or triple bond and a silane reagent, characterized in that, The unsaturated compound is allyl glycidyl ether, 1-octene, 2-methyl-3-butyn-2-ol, or styrene; the silane reagent is trimethoxysilane; and the molar ratio of the unsaturated compound to trimethoxysilane is 1:1-1.
5.
7. The application according to claim 6, characterized in that, The reaction temperature is 60-80℃; the reaction time is 8-12h; the reaction solvent is a hydrocarbon solvent; and the reaction atmosphere is an inert gas.
Citation Information
Patent Citations
N-heterocyclic carbene platinum complex metal carboxylate integrated catalyst and preparation method thereof
CN104324752A
Sulfoxide platinum tetramethyl divinyl siloxane complex for catalyzing hydrosilylation reaction and synthesis method of sulfoxide platinum tetramethyl divinyl siloxane complex
CN116606324A