The traditional TC4 titanium alloy is close to its use limit in additive manufacturing, and it is difficult to further improve its strength and heat resistance.
By mixing TC4 titanium alloy powder with aluminum powder and performing ball milling in a low-temperature ball milling tank, followed by heat treatment in a heating device to form β phase, combined with photoelectric means to excite titanium dioxide, and coating graphene to enhance the strength of titanium alloy powder and hardness.
It significantly improves the strength and toughness of titanium alloy powder, forms a beta phase with high strength and toughness, and enhances its performance through a graphene coating layer, making it suitable for additive manufacturing of complex structures.
Smart Images

Figure BDA0004796319090000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field, and in particular to a titanium alloy powder for additive manufacturing and a preparation method thereof. Background Art
[0002] Additive manufacturing technology is a rapid prototyping technology based on the concept of discrete accumulation. Its core is to gradually build a three-dimensional object by stacking or adding materials layer by layer, rather than cutting or removing materials from a block of material to obtain the desired shape. Additive manufacturing technology can produce a variety of large and complex parts. Compared with traditional processing methods, it reduces the amount of mechanical processing and can greatly increase the processing speed.
[0003] Titanium alloy is a widely used lightweight material in the field of aerospace due to its low density, high specific strength, high temperature resistance, corrosion resistance, and non-magnetic properties. TC4 alloy is a medium-strength α-β two-phase titanium alloy containing 6% α-stabilizing element Al and 4% β-stabilizing element V. The alloy can work at a temperature of up to 400°C for a long time. In the aviation industry, it is mainly used to manufacture engine fans and compressor discs and blades, as well as important load-bearing components such as beams, joints and bulkheads in aircraft structures. However, with the development of technology and changes in the application environment, traditional TC4 titanium alloy has gradually approached its limit of use. Composite materials of TC4 titanium alloy to improve its strength and heat resistance will be the focus of future research. Summary of the invention
[0004] In order to solve at least one of the above problems, the present application provides a method for preparing titanium alloy powder for additive manufacturing, comprising the following steps: S10: mixing TC4 titanium alloy powder and aluminum powder to obtain a mixed metal powder; wherein the particle size of the aluminum powder is smaller than that of the TC4 titanium alloy powder; S20: under a protective atmosphere, placing the mixed metal powder into a low-temperature ball mill for ball milling to obtain a composite metal powder; S30: using a protective atmosphere to blow the composite metal powder into a first heating device, a second heating device, and a cooling device in sequence, and collect to obtain a titanium alloy powder; wherein the temperature of the second heating device is greater than the temperature of the first heating device.
[0005] Furthermore, the particle sizes of TC4 titanium alloy powder and aluminum powder satisfy R / r≥100; wherein 2R is the particle size of TC4 titanium alloy powder, 2r is the particle size of aluminum powder; and the mass ratio of TC4 titanium alloy powder to aluminum powder is ρ1R 3 :A·ρ2(3Rr 2 +3R 2 r+8r 3 ). Wherein, ρ1 is the density of TC4 titanium alloy powder; ρ2 is the density of aluminum powder; A is a coefficient, ranging from 0.2 to 1.8, preferably from 0.5 to 1.0.
[0006] Furthermore, step S20 includes: S21: placing a ball milling medium in a low-temperature ball mill, and introducing a protective atmosphere to replace the gas in the low-temperature ball mill; S22: placing the mixed metal powder in the low-temperature ball mill, and setting the ball milling temperature to between -100°C and -60°C; S23: ball milling the low-temperature ball mill in a planetary ball mill at a speed of 700-800rpm for 2-3h; after the ball milling is completed, a composite metal powder is obtained.
[0007] Furthermore, the ball milling medium is zirconia beads; the ball milling medium includes 3 mm zirconia beads and 5 mm zirconia beads, wherein the ratio of 3 mm zirconia beads to 5 mm zirconia beads added is (2-4):1; the ball-to-material ratio is (4-8):1.
[0008] Furthermore, the temperature of the first heating device is controlled to be 600-660°C, and the temperature of the second heating device is controlled to be 880-890°C; the speed of the protective atmosphere is controlled so that the movement time of the composite metal powder in the first heating device is 30-45 minutes, and the movement time in the second heating device is 45-60 minutes. The cooling device includes a first cooling section and a second cooling section, wherein the temperature of the first cooling section is room temperature; the temperature of the second cooling section is -10±5°C.
[0009] Furthermore, the method for preparing the titanium alloy powder also includes: S40: coating the surface of the titanium alloy powder with graphene to obtain graphene-reinforced titanium alloy powder.
[0010] Furthermore, step S40 includes: S41: dispersing nano titanium dioxide and monolayer graphene in an organic solvent to obtain a mixture A; S42: applying ultrasonic vibration to the mixture A and adding titanium alloy powder to obtain a mixture B; S43: irradiating the mixture B with an ultraviolet lamp and adding an electrode at the same time, controlling the current to 4-6 mA, and reacting for 3-4 hours to obtain a mixture C; S44: washing and drying the mixture C, and then heat-insulating it in a vacuum environment to obtain a graphene-enhanced titanium alloy powder.
[0011] Furthermore, the organic solvent is tetrahydrofuran; the power of the ultrasonic vibration is 80-100 kHz; the wavelength of the ultraviolet lamp is 340-380 nm; the vacuum degree of the vacuum environment is 1×10 -3 -1×10 -2 Pa, the temperature of the insulation treatment is 600-800℃, and the insulation time is 3-4h.
[0012] The present application also provides a titanium alloy powder for additive manufacturing, which is prepared by the above method.
[0013] The present invention selects aluminum powder to strengthen TC4 titanium alloy powder; firstly, the aluminum powder and TC4 titanium alloy powder are mechanically combined by mechanical ball milling, and then the composite metal powder is blown into two heating devices in sequence. As the heating temperature increases, the aluminum powder in the composite metal powder can be dissolved to form a β phase under the action of high temperature, thereby improving the strength and hardness of the TC4 titanium alloy powder. After the composite metal powder enters the first heating device, the aluminum powder on the surface becomes a molten state under the action of high temperature. Based on the effect of surface tension, the sphericity of the composite metal powder can be further improved. At the same time, aluminum and titanium can form a stable sub-compound, and then enter the second heating device, and keep it at a temperature of 880-890°C for 45-60 minutes. Combined with the rapid cooling process, a high-strength and high-toughness β phase can be obtained. On the other hand, photoelectric means are used to excite titanium dioxide to produce holes, and the holes are further used to adsorb graphene and titanium alloy powder in the reaction system; thereby combining to obtain graphene-enhanced titanium alloy powder. The graphene-enhanced titanium alloy powder has a three-layer structure, including a core, a transition layer and an outer shell from the inside to the outside, wherein the core is TC4 titanium alloy powder, the transition layer is an Al-Ti subcompound, and the outer shell is a coating layer of titanium dioxide and graphene. DETAILED DESCRIPTION
[0014] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] In the related technology, TC4 titanium alloy powder is a medium-strength α-β two-phase titanium alloy; α is a stable phase that affects the tensile plasticity and fatigue properties of titanium alloys. Generally speaking, the more α phases there are, the better the ductility and fatigue properties of titanium alloys; β phase is a high-temperature phase formed above 800°C, which can improve the strength, hardness and thermal stability of titanium alloys. TC4 titanium alloy achieves performance improvements in many aspects such as strength and thermal stability by adding 6% aluminum and 4% vanadium.
[0016] However, with the change of the use environment, TC4 titanium alloy is getting closer and closer to its use limit when applied to additive manufacturing. The relevant technologies also involve a lot of various modification treatments for TC4 titanium alloy to improve its strength and other properties. For example, the surface of TC4 titanium alloy is coated with reinforcing materials such as ceramics and tungsten carbide; however, these technical solutions are often easy to obtain irregular powder particles when processing TC4 titanium alloy. Since the particle size of titanium alloy powder itself is very small, some very slight deviations can easily cause the particle size of titanium alloy powder to change greatly during the coating process.
[0017] In order to solve the above problems, an embodiment of the present application provides a method for preparing titanium alloy powder for additive manufacturing, comprising the following steps: S10: mixing TC4 titanium alloy powder and aluminum powder to obtain a mixed metal powder; wherein the particle size of the aluminum powder is smaller than that of the TC4 titanium alloy powder; S20: under a protective atmosphere, placing the mixed metal powder in a low-temperature ball mill for ball milling to obtain a composite metal powder; S30: using a protective atmosphere to blow the composite metal powder into a first heating device, a second heating device, and a cooling device in sequence to collect the titanium alloy powder; wherein the temperature of the second heating device is greater than the temperature of the first heating device.
[0018] In this embodiment, aluminum powder is selected to strengthen the TC4 titanium alloy powder; first, the aluminum powder and the TC4 titanium alloy powder are mechanically combined by mechanical ball milling, and then the composite metal powder is blown into two heating devices in sequence. As the heating temperature increases, the aluminum powder in the composite metal powder can be dissolved under high temperature to form a β phase, thereby improving the strength and hardness of the TC4 titanium alloy powder.
[0019] Furthermore, the particle sizes of TC4 titanium alloy powder and aluminum powder satisfy R / r≥100; wherein 2R is the particle size of TC4 titanium alloy powder, 2r is the particle size of aluminum powder; and the mass ratio of TC4 titanium alloy powder to aluminum powder is ρ1R 3 :A·ρ2(3Rr 2 +3R 2 r+8r 3 ). Wherein, ρ1 is the density of TC4 titanium alloy powder; ρ2 is the density of aluminum powder; A is a coefficient, ranging from 0.2 to 1.8, preferably from 0.5 to 1.0.
[0020] In this embodiment, the particle size 2R of the TC4 titanium alloy powder can be 20μm, 60μm, 100μm, 200μm or other, and the particle size 2r of the aluminum powder needs to meet the following conditions: R / r≥100, so that the aluminum powder can be coated on the surface of the TC4 titanium alloy powder. On the other hand, the amount of aluminum powder added is also crucial. Too little aluminum powder cannot achieve uniform coating on the surface of the TC4 titanium alloy powder. Too much aluminum powder will affect the performance of the alloy. Only an appropriate amount of aluminum powder can effectively improve the strength and hardness of the TC4 titanium alloy powder; therefore, a limit is given to the amount of aluminum powder added, where A is a coefficient, and technicians in this field can adjust it according to actual needs.
[0021] Furthermore, step S20 includes: S21: placing a ball milling medium in a low-temperature ball mill, and introducing a protective atmosphere to replace the gas in the low-temperature ball mill; S22: placing the mixed metal powder in the low-temperature ball mill, and setting the ball milling temperature to between -100°C and -60°C; S23: ball milling the low-temperature ball mill in a planetary ball mill at a speed of 700-800rpm for 2-3h; after the ball milling is completed, a composite metal powder is obtained.
[0022] In this embodiment, protective gas needs to be passed during ball milling, and the ball milling temperature is controlled between -100°C and -60°C; oxidation of the alloy can be effectively avoided. In the related art, the rotation speed used for ball milling of aluminum powder is generally not too high. In order to protect the sphericity of the aluminum powder, a low-speed and long-term ball milling strategy is adopted, such as ball milling at a speed of 300rpm for 5h. However, in this embodiment, since the composite metal powder will be further post-processed, the ball milling speed is set at 700-800rpm for 2-3 hours to quickly mix the aluminum powder and TC4 titanium alloy powder.
[0023] Furthermore, the ball milling medium is zirconia beads; the ball milling medium includes 3 mm zirconia beads and 5 mm zirconia beads, wherein the ratio of 3 mm zirconia beads to 5 mm zirconia beads added is (2-4):1; the ball-to-material ratio is (4-8):1.
[0024] In this embodiment, since the particle sizes of aluminum powder and TC4 titanium alloy powder are very small, zirconium oxide beads with smaller particle sizes are also selected as the ball milling medium. Small balls (3mm zirconium oxide beads) are mainly used for ball milling, and a certain number of large balls (5mm zirconium oxide beads) are matched; during the ball milling process, the small balls and the large balls are constantly impacted, and based on the addition ratio of the two balls and the setting of the ball-to-material ratio, the number of impacts is large, and the impact force is small, so that the aluminum powder and the TC4 titanium alloy powder can be mechanically combined under continuous small-force impacts, and finally the TC4 titanium alloy powder with aluminum powder coated on the surface is obtained, that is, the composite metal powder.
[0025] Furthermore, the temperature of the first heating device is controlled to be 600-660°C, and the temperature of the second heating device is controlled to be 880-890°C; the speed of the protective atmosphere is controlled so that the movement time of the composite metal powder in the first heating device is 30-45 minutes, and the movement time in the second heating device is 45-60 minutes. The cooling device includes a first cooling section and a second cooling section, wherein the temperature of the first cooling section is room temperature; the temperature of the second cooling section is -10±5°C.
[0026] In this embodiment, the composite metal powder is mechanically combined with the TC4 titanium alloy powder due to ball milling before entering the first heating device, and its structure is TC4 titanium alloy powder with aluminum powder coated on the surface. Therefore, when the composite metal powder enters the first heating device, the aluminum powder on the surface becomes molten under the action of high temperature, and the sphericity of the composite metal powder can be further improved based on the effect of surface tension. At the same time, aluminum and titanium can form a stable sub-compound, and then enter the second heating device, keep it at 880-890℃ for 45-60 minutes, and combine it with rapid cooling to obtain a high-strength and high-toughness β phase.
[0027] Furthermore, the method for preparing the titanium alloy powder also includes: S40: coating the surface of the titanium alloy powder with graphene to obtain graphene-reinforced titanium alloy powder.
[0028] In this embodiment, in order to further improve the strength of the titanium alloy powder, graphene is coated on its surface. During laser additive manufacturing, the graphene in the graphene-enhanced titanium alloy powder can react with aluminum and titanium to generate Al2O3 and TiC in situ, thereby obtaining dual-phase reinforcement.
[0029] Furthermore, step S40 includes: S41: dispersing nano titanium dioxide and monolayer graphene in an organic solvent to obtain a mixture A; S42: applying ultrasonic vibration to the mixture A and adding titanium alloy powder to obtain a mixture B; S43: irradiating the mixture B with an ultraviolet lamp and adding an electrode at the same time, controlling the current to 4-6 mA, and reacting for 3-4 hours to obtain a mixture C; S44: washing and drying the mixture C, and then heat-insulating it in a vacuum environment to obtain a graphene-enhanced titanium alloy powder.
[0030] Wherein, the mass ratio of nano titanium dioxide, single-layer graphene and titanium alloy powder is (1-5): (1-5):100.
[0031] Titanium dioxide is a photosensitive wide-band semiconductor material. When it is exposed to light with a wavelength less than 387nm, the electrons in its valence band will be excited and migrate to the surface of the titanium dioxide particles, and holes will be formed in the valence band. Therefore, in this embodiment, titanium dioxide and a single layer of graphene are first dispersed evenly, and then titanium alloy powder is added, and holes are generated in titanium dioxide through photoelectric stimulation, and the holes are further used to adsorb the graphene and titanium alloy powder in the reaction system; thereby, graphene-enhanced titanium alloy powder is obtained.
[0032] Furthermore, the organic solvent is tetrahydrofuran; the power of the ultrasonic vibration is 80-100 kHz; the wavelength of the ultraviolet lamp is 340-380 nm; the vacuum degree of the vacuum environment is 1×10 -3 -1×10 -2 Pa, the temperature of the insulation treatment is 600-800℃, and the insulation time is 3-4h.
[0033] The present application also provides a titanium alloy powder for additive manufacturing, which is prepared by the above method.
[0034] Example 1
[0035] A method for preparing titanium alloy powder for additive manufacturing comprises the following steps:
[0036] S10: Mixing TC4 titanium alloy powder and aluminum powder to obtain mixed metal powder; wherein the particle size of the aluminum powder is smaller than that of the TC4 titanium alloy powder.
[0037] The particle sizes of TC4 titanium alloy powder and aluminum powder satisfy R / r=100; wherein 2R is the particle size of TC4 titanium alloy powder, and 2r is the particle size of aluminum powder; the mass ratio of TC4 titanium alloy powder to aluminum powder is ρ1R 3 :A·ρ2(3Rr 2 +3R 2 r+8r 3 ). Among them, ρ1 is the density of TC4 titanium alloy powder; ρ2 is the density of aluminum powder; A is the coefficient, and the value range is 0.2.
[0038] S20: Under a protective atmosphere, the mixed metal powder is placed in a low-temperature ball mill for ball milling to obtain a composite metal powder.
[0039] S21: Put ball milling media into a low-temperature ball mill, and introduce protective atmosphere to replace the gas in the low-temperature ball mill; the ball milling media is zirconia beads; the ball milling media includes 3mm zirconia beads and 5mm zirconia beads, wherein the ratio of 3mm zirconia beads to 5mm zirconia beads is 4:1; the ball-to-material ratio is 8:1.
[0040] S22: Put the mixed metal powder into a low-temperature ball mill and set the ball milling temperature to between -100°C and -60°C.
[0041] S23: The low-temperature ball mill is subjected to ball milling treatment at a rotation speed of 700 rpm in a planetary ball mill for 3 hours; after the ball milling is completed, a composite metal powder is obtained.
[0042] S30: using a protective atmosphere to blow the composite metal powder into a first heating device, a second heating device, and a cooling device in sequence, and collecting the titanium alloy powder; wherein the temperature of the second heating device is greater than the temperature of the first heating device.
[0043] The temperature of the first heating device is controlled to be 660°C, and the temperature of the second heating device is controlled to be 890°C; the speed of the protective atmosphere is controlled so that the movement time of the composite metal powder in the first heating device is 45 minutes, and the movement time in the second heating device is 60 minutes. The cooling device includes a first cooling section and a second cooling section, wherein the temperature of the first cooling section is room temperature; the temperature of the second cooling section is -15°C.
[0044] S41: dispersing nano-titanium dioxide and monolayer graphene in tetrahydrofuran to obtain a mixture A.
[0045] S42: applying ultrasonic vibration to mixture A, wherein the power of the ultrasonic vibration is 100 kHz; and adding titanium alloy powder at the same time to obtain mixture B.
[0046] S43: Using an ultraviolet lamp to irradiate the mixture B, the wavelength of the ultraviolet lamp is 380nm; adding electrodes at the same time, controlling the current to 6mA, and obtaining the mixture C after reacting for 4 hours.
[0047] S44: After washing and drying the mixture C, heat preservation treatment is carried out in a vacuum environment to obtain graphene-enhanced titanium alloy powder. The vacuum degree of the vacuum environment is 1×10 -2 Pa, the temperature of the insulation treatment is 800℃, and the insulation time is 4h.
[0048] Wherein, the mass ratio of nano titanium dioxide, single-layer graphene and titanium alloy powder is (1-5): (1-5):100.
[0049] Example 2
[0050] This embodiment provides a method for preparing titanium alloy powder for additive manufacturing. The preparation method thereof is similar to that of Embodiment 1, except that:
[0051] In step S10, R / r=120, and A takes a value of 1.8.
[0052] Example 3
[0053] This embodiment provides a method for preparing titanium alloy powder for additive manufacturing. The preparation method thereof is similar to that of Embodiment 1, except that:
[0054] In step S21, the ratio of 3 mm zirconia beads to 5 mm zirconia beads added is 2:1; the ball-to-material ratio is 4:1.
[0055] In step S23, the low-temperature ball milling jar is subjected to ball milling treatment at a rotation speed of 800 rpm for 2 hours in a planetary ball mill; after the ball milling is completed, a composite metal powder is obtained.
[0056] Example 4
[0057] This embodiment provides a method for preparing titanium alloy powder for additive manufacturing. The preparation method thereof is similar to that of Embodiment 1, except that:
[0058] In step S30, the temperature of the first heating device is controlled to be 600°C, and the temperature of the second heating device is controlled to be 880°C; the speed of the protective atmosphere is controlled so that the movement time of the composite metal powder in the first heating device is 30 minutes, and the movement time in the second heating device is 45 minutes. The cooling device includes a first cooling section and a second cooling section, wherein the temperature of the first cooling section is room temperature; the temperature of the second cooling section is -5°C.
[0059] Example 5
[0060] This embodiment provides a method for preparing titanium alloy powder for additive manufacturing. The preparation method thereof is similar to that of Embodiment 1, except that:
[0061] In step S42, the power of the ultrasonic vibration is 80 kHz.
[0062] In step S43, the wavelength of the UV lamp is 340nm; the current is 4mA, and the reaction time is 3 hours.
[0063] In step S44, the vacuum degree of the vacuum environment is 1×10 -3 Pa, the temperature of the insulation treatment is 600℃, and the insulation time is 3h.
[0064] Comparative Example 1
[0065] This embodiment provides a method for preparing titanium alloy powder for additive manufacturing. The preparation method thereof is similar to that of Embodiment 1, except that the processing of S41-S44 is not performed.
[0066] Comparative Example 2
[0067] This embodiment provides a method for preparing titanium alloy powder for additive manufacturing. The preparation method thereof is similar to that of Embodiment 1, except that: the S10-S30 treatment is not performed, and TC4 titanium alloy powder is directly used as raw material, and graphene is coated on its surface.
[0068] The titanium alloy powder provided in the embodiment and the comparative example was used for laser printing, and the performance of the printed standard samples was tested. The test results are shown in Table 1.
[0069]
[0070] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing titanium alloy powder for additive manufacturing, It is characterized in that The following steps are involved: S10: mixing TC4 titanium alloy powder and aluminum powder to obtain mixed metal powder; wherein the particle size of the aluminum powder is smaller than that of the TC4 titanium alloy powder; S20: placing the mixed metal powder into a low-temperature ball mill under a protective atmosphere for ball milling to obtain a composite metal powder; S30: using a protective atmosphere to sequentially blow the composite metal powder into a first heating device, a second heating device, and a cooling device to collect the titanium alloy powder; wherein the temperature of the second heating device is greater than the temperature of the first heating device; Controlling the temperature of the first heating device to 600-660° C. and the temperature of the second heating device to 880-890° C.; Controlling the speed of the protective atmosphere so that the composite metal powder moves for 30-45 minutes in the first heating device and for 45-60 minutes in the second heating device; The cooling device comprises a first cooling section and a second cooling section, wherein the temperature of the first cooling section is room temperature; and the temperature of the second cooling section is -10±5°C.
2. The method for preparing the titanium alloy powder according to claim 1, It is characterized in that The particle sizes of the TC4 titanium alloy powder and the aluminum powder satisfy R / r≥100; Wherein, 2R is the particle size of the TC4 titanium alloy powder, and 2r is the particle size of the aluminum powder; The mass ratio of the TC4 titanium alloy powder to the aluminum powder is ρ 1 R 3 :A·ρ 2 (3Rr 2 +3R 2 r+8r 3 ); Among them, ρ 1 is the density of the TC4 titanium alloy powder; ρ 2 is the density of the aluminum powder; A is a coefficient, and its value range is 0.2-1.
8.
3. The method for preparing the titanium alloy powder according to claim 1, It is characterized in that Step S20 includes: S21: placing a ball milling medium in the low-temperature ball mill, and introducing a protective atmosphere to replace the gas in the low-temperature ball mill; S22: placing the mixed metal powder into the low-temperature ball milling tank, and setting the ball milling temperature to between -100° C. and -60° C.; S23: ball milling the low-temperature ball mill in a planetary ball mill at a rotation speed of 700-800 rpm for 2-3 hours; after the ball milling is completed, the composite metal powder is obtained.
4. The method for preparing titanium alloy powder according to claim 1, It is characterized in that The ball milling medium is zirconia beads; the ball milling medium includes 3 mm zirconia beads and 5 mm zirconia beads; The ratio of the 3 mm zirconia beads to the 5 mm zirconia beads is (2-4): 1; The ball-to-material ratio of the ball milling process is (4-8):
1.
5. The method for preparing the titanium alloy powder according to any one of claims 1 to 4, It is characterized in that Also includes: S40: coating the surface of the titanium alloy powder with graphene to obtain graphene-enhanced titanium alloy powder.
6. The method for preparing titanium alloy powder according to claim 5, It is characterized in that Step S40 includes: S41: dispersing nano-titanium dioxide and monolayer graphene in an organic solvent to obtain a mixture A; S42: applying ultrasonic vibration to the mixture A and adding the titanium alloy powder to obtain a mixture B; S43: irradiating the mixture B with an ultraviolet lamp, adding electrodes at the same time, controlling the current to 4-6 mA, and reacting for 3-4 hours to obtain a mixture C; S44: After washing and drying the mixture C, heat-insulating treatment is performed under a vacuum environment to obtain the graphene-enhanced titanium alloy powder.
7. The method for preparing titanium alloy powder according to claim 6, It is characterized in that The organic solvent is tetrahydrofuran; The power of the ultrasonic vibration is 80-100kHz; The wavelength of the ultraviolet lamp is 340-380nm; The vacuum degree of the vacuum environment is 1×10 -3 -1×10 -2 Pa; The temperature of the heat preservation treatment is 600-800° C., and the heat preservation time is 3-4 hours.
8. A titanium alloy powder for additive manufacturing, It is characterized in that The titanium alloy powder is prepared by the method according to any one of claims 1 to 7.