A thermally conductive graphene sheet and preparation method thereof
By coating both sides of the glass fiber sheet with a silicone surface-modified graphene microchip rubber layer and filling it with boron nitride, the problem of graphene sheet toughness and poor vertical thermal conductivity is solved, achieving efficient thermal conductivity and low thermal conductivity. resistance, suitable for a variety of applications.
Patent Information
- Application Number
- CN202410695430.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-05-31
AI Technical Summary
The poor toughness, rough surface and poor vertical thermal conductivity of conventional graphene sheets limit their application in the fields of assembly and thermal management.
By coating both sides of the glass fiber sheet with a silicone surface-modified graphene microsheet rubber layer and filling it with boron nitride during the hot pressing process, the interlayer structure of the graphene microsheets is optimized and the toughness and thermal conductivity of the material are increased. .
It improves the toughness and vertical thermal conductivity of graphene sheets, reduces contact thermal resistance, and enhances thermal conductivity efficiency. It is suitable for thermal management, electronic device heat dissipation and new energy fields.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the field of graphene, and in particular relates to a thermally conductive graphene sheet and a preparation method thereof. Background Art
[0002] Graphene is a two-dimensional crystal structure composed of carbon atoms with excellent thermal conductivity. However, conventional graphene sheets have some problems in some applications. First, conventional graphene sheets have poor toughness and are prone to cracking during bending, affecting their assembly performance. Second, the surface of conventional graphene sheets is relatively rough, resulting in high contact thermal resistance. Finally, conventional graphene sheets have high in-plane thermal conductivity, but poor vertical thermal conductivity, which limits their effectiveness in some vertical thermal conductivity applications.
[0003] Therefore, it is necessary to develop a new type of thermally conductive graphene sheet to solve the problems of poor toughness, rough surface and poor vertical thermal conductivity of conventional graphene sheets in the prior art. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a thermally conductive graphene sheet and a preparation method thereof. The thermally conductive graphene sheet provided by the present invention has good toughness, a smooth surface, and excellent in-plane thermal conductivity and vertical thermal conductivity.
[0005] The present invention provides a thermally conductive graphene sheet, which is made by hot pressing a thermally conductive graphene sheet semi-finished product. The thermally conductive graphene sheet semi-finished product comprises a glass fiber sheet and a graphene microsheet adhesive layer composited on both side surfaces of the glass fiber sheet. The components of the graphene microsheet adhesive layer include organic silicon surface modified graphene microsheets, boron nitride and organic silica gel water.
[0006] Preferably, the particle size (equivalent diameter) of the graphene microplatelets in the organosilicon surface-modified graphene microplatelets is 30-100 μm.
[0007] Preferably, the particle size of the boron nitride is 30-100 μm.
[0008] Preferably, the mass ratio of the organic silicon surface modified graphene microsheets, boron nitride and organic silicon water is 80: (5-30): (20-80).
[0009] Preferably, the thickness of the glass fiber sheet is 10-50 μm; the thickness of the graphene microsheet adhesive layer on one side of the glass fiber sheet is 50-200 μm.
[0010] The present invention provides a method for preparing the thermally conductive graphene sheet described in the above technical solution, comprising the following steps:
[0011] a) mixing organic silicon surface modified graphene microsheets, boron nitride, organic silicon water and solvent to obtain graphene microsheet rubber material;
[0012] b) coating the graphene microsheet sizing material on both sides of the glass fiber sheet and drying the sizing material to obtain a semi-finished thermally conductive graphene sheet;
[0013] c) hot-pressing the semi-finished thermally conductive graphene sheet to obtain a thermally conductive graphene sheet.
[0014] Preferably, in step a), the organosilicon surface-modified graphene microsheets are prepared according to the following steps: soaking the graphene microsheet raw material in an organosilicon modifier, taking out and drying, to obtain the organosilicon surface-modified graphene microsheets.
[0015] Preferably, the graphene microplatelet raw material is prepared according to the following steps: graphite powder is acid-washed to obtain the graphene microplatelet raw material.
[0016] Preferably, in step a), the specific process of mixing includes: firstly mixing the organic silicon surface modified graphene microsheets and a solvent to obtain a graphene microsheet slurry; and then mixing the graphene microsheet slurry, boron nitride and organic silicon water to obtain a graphene microsheet slurry.
[0017] Preferably, in step c), the hot pressing pressure is 5-15 MPa; the hot pressing temperature is 140-180°C.
[0018] Compared with the prior art, the present invention provides a thermally conductive graphene sheet and a preparation method thereof. The thermally conductive graphene sheet provided by the present invention is made by hot pressing a thermally conductive graphene sheet semi-finished product, wherein the thermally conductive graphene sheet semi-finished product comprises a glass fiber sheet and a graphene micro-sheet adhesive layer composited on both sides of the glass fiber sheet, wherein the components of the graphene micro-sheet adhesive layer include organic silicon surface modified graphene micro-sheets, boron nitride and organic silica gel water. The present invention increases the wettability and fillability of graphene microsheets and improves the toughness of thermally conductive graphene sheets by modifying the surface of graphene microsheets with organic silicon; by filling boron nitride between the gaps of graphene microsheet powder, the interlayer structure of graphene microsheets is optimized, not only can the surface of the sheet after molding be smooth and flat, but also the longitudinal heat conduction channel of the material can be increased, and the vertical thermal conductivity of the graphene sheet can be improved; by sandwiching the glass fiber sheet as a reinforcing layer in the middle of the thermally conductive graphene sheet, the toughness and strength of the sheet are further improved; by using the hot pressing method to compound the semi-finished material, it is combined into a dense whole, the internal structure of the sheet is optimized, the interlayer resistance is reduced, and the thermal conductivity of the sheet is further increased. The thermally conductive graphene sheet provided by the present invention has good toughness, a smooth surface, and takes into account excellent in-plane thermal conductivity and vertical thermal conductivity, and has broad application prospects in the application fields such as thermal management, electronic device heat dissipation, and new energy fields. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] The present invention provides a thermally conductive graphene sheet, which is made by hot pressing a thermally conductive graphene sheet semi-finished product. The thermally conductive graphene sheet semi-finished product comprises a glass fiber sheet and a graphene microsheet adhesive layer composited on both side surfaces of the glass fiber sheet. The components of the graphene microsheet adhesive layer include organic silicon surface modified graphene microsheets, boron nitride and organic silica gel water.
[0021] In the thermally conductive graphene sheet provided by the present invention, the thickness of the glass fiber sheet is preferably 10-50 μm, specifically 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.
[0022] In the thermally conductive graphene sheet provided by the present invention, in the graphene microsheet rubber layer, the organosilicon surface modified graphene microsheet is preferably prepared according to the following steps: soaking the graphene microsheet raw material in the organosilicon modifier, taking it out and drying it, and obtaining the organosilicon surface modified graphene microsheet. Wherein, the particle size of the graphene microsheet raw material is preferably 30~100μm, specifically 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm or 100μm; the soaking temperature is preferably 10~40℃, specifically 10℃, 15℃, 20℃, 25℃, 30℃, 35℃ or 40℃; the soaking time is preferably 10~60min, specifically 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min.
[0023] In the thermally conductive graphene sheet provided by the present invention, in the graphene microsheet rubber layer, the particle size of the boron nitride is preferably 30-100 μm, specifically 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.
[0024] In the thermally conductive graphene sheet provided by the present invention, in the graphene microsheet sizing layer, the mass ratio of the organic silicon surface modified graphene microsheet, boron nitride and organic silica gel water is preferably 80: (5-30): (20-80), wherein the mass ratio of the organic silicon surface modified graphene microsheet and boron nitride can be specifically 80:5, 80:6, 80:7, 80:8, 80:9, 80:10, 80:11, 80:12, 80:13, 80:14, 80:15, 80:16, 80:17, 80:18 8, 80:19, 80:20, 80:21, 80:22, 80:23, 80:24, 80:25, 80:26, 80:27, 80:28, 80:29 or 80:30; the mass ratio of the organic silicon surface modified graphene microsheets and the organic silicon water can be 80:20, 80:25, 80:30, 80:35, 80:40, 80:45, 80:50, 80:55, 80:60, 80:65, 80:70, 80:75 or 80:80.
[0025] In the thermally conductive graphene sheet provided by the present invention, the single-side thickness of the graphene microsheet glue layer is preferably 50-200 μm, specifically 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm or 200 μm.
[0026] In the thermally conductive graphene sheet provided by the present invention, the hot pressing pressure is preferably 5-15 MPa, specifically 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa or 15 MPa; the hot pressing temperature is preferably 140-180°C, specifically 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C; the hot pressing time is preferably 30-180s, specifically 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, 160s, 170s or 180s.
[0027] The present invention also provides a method for preparing the thermally conductive graphene sheet described in the above technical solution, comprising the following steps:
[0028] a) mixing organic silicon surface modified graphene microsheets, boron nitride, organic silicon water and solvent to obtain graphene microsheet rubber material;
[0029] b) coating the graphene microsheet sizing material on both sides of the glass fiber sheet and drying the sizing material to obtain a semi-finished thermally conductive graphene sheet;
[0030] c) hot-pressing the semi-finished thermally conductive graphene sheet to obtain a thermally conductive graphene sheet.
[0031] In the preparation method provided by the present invention, in step a), the organic silicon surface modified graphene micro-sheet is preferably prepared according to the following steps: soaking the graphene micro-sheet raw material in the organic silicon modifier, taking it out and drying it, and obtaining the organic silicon surface modified graphene micro-sheet. Wherein, the particle size of the graphene micro-sheet raw material is preferably 30-100 μm, specifically 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm; the soaking temperature is preferably 10-40°C, specifically 10°C, 15°C, 20°C, 25°C, 30°C, 35°C or 40°C; the soaking time is preferably 10-60min, specifically 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min.
[0032] In the preparation method provided by the present invention, the graphene microplatelet raw material is preferably prepared according to the following steps: acid-washing graphite powder to obtain graphene microplatelet raw material. In the present invention, the graphene microplatelet raw material obtained by acid-washing is preferably screened to obtain graphene microplatelet raw material of required size.
[0033] In the preparation method provided by the present invention, in step a), the particle size of the boron nitride is preferably 30-100 μm, specifically 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.
[0034] In the preparation method provided by the present invention, in step a), the mass ratio of the organic silicon surface modified graphene microsheets, boron nitride and organic silica gel water is preferably 80: (5-30): (20-80), wherein the mass ratio of the organic silicon surface modified graphene microsheets and boron nitride can be specifically 80:5, 80:6, 80:7, 80:8, 80:9, 80:10, 80:11, 80:12, 80:13, 80:14, 80:15, 80:16, 80:17, 80:18, 80:19, 80:20, 80:21, 80:22, 80:23, 80:24, 80:25, 80:26, 80:27, 80:28, 80:29, 80:30, 80:31, 80:32, 80:33, 80:34, 80:35, 80:36, 80:37, 80:38, 80:39, 80:40, 80:41, 80:42, 80:43, 80:44, 80:45, 80:46, 80:47, 80:48, 80:49, 80:50, 80:51, 80:52, 80:53, 80:54, 80:55 : The mass ratio of the organic silicon surface modified graphene microsheets and the organic silicon water can be 80:20, 80:25, 80:30, 80:35, 80:40, 80:45, 80:50, 80:55, 80:60, 80:65, 80:70, 80:75 or 80:80.
[0035] In the preparation method provided by the present invention, in step a), there is no particular limitation on the type and amount of the solvent, and the organic silicon surface modified graphene microsheets, boron nitride and organic silicon water can be uniformly mixed and dispersed, and a benzene solvent is preferably used.
[0036] In the preparation method provided by the present invention, in step a), the mixing temperature is preferably 10-40°C, more preferably 25°C (room temperature); the specific mixing process preferably includes: a1) first mixing the organic silicon surface modified graphene microsheets and the solvent to obtain the graphene microsheet slurry; a2) then mixing the graphene microsheet slurry, boron nitride and organic silica gel water to obtain the graphene microsheet sizing material. Wherein, the mixing method in step a1) is preferably first ultrasonic mixing, then stirring and mixing, and finally continuing ultrasonic mixing, the first ultrasonic mixing time is preferably 10-15min, the stirring and mixing time is preferably 30-40min, and the second ultrasonic mixing time is preferably 10-15min; the mixing method in step a2) is preferably first ultrasonic mixing, then stirring and mixing, and finally continuing ultrasonic mixing, the first ultrasonic mixing time is preferably 10-15min, the stirring and mixing time is preferably 30-40min, and the second ultrasonic mixing time is preferably 10-15min.
[0037] In the preparation method provided by the present invention, in step b), the thickness of the glass fiber sheet is preferably 10-50 μm, specifically 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm.
[0038] In the preparation method provided by the present invention, in step b), the coating method is preferably blade coating; the single-side dry coating thickness of the graphene microsheet rubber on the glass fiber sheet is preferably 50-200 μm, specifically 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm or 200 μm.
[0039] In the preparation method provided by the present invention, in step c), the hot pressing pressure is preferably 5-15 MPa, specifically 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa or 15 MPa; the hot pressing temperature is preferably 140-180°C, specifically 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C; the hot pressing time is preferably 30-180s, specifically 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, 160s, 170s or 180s.
[0040] The technical solution provided by the present invention increases the wettability and fillability of the graphene microsheets and improves the toughness of the thermally conductive graphene sheets by modifying the surfaces of the graphene microsheets with organic silicon; optimizes the interlayer structure of the graphene microsheets by filling boron nitride between the gaps between the graphene microsheet powders, which not only makes the surface of the formed sheet smooth and flat, but also increases the longitudinal heat conduction channels of the material and improves the vertical thermal conductivity of the graphene sheets; further improves the toughness and strength of the sheets by sandwiching the glass fiber sheets as reinforcement layers in the middle of the thermally conductive graphene sheets; and composites the semi-finished materials by hot pressing to form a dense whole, thereby optimizing the internal structure of the sheets, reducing interlayer resistance and further increasing the thermal conductivity of the sheets.
[0041] The technical solution provided by the present invention has at least the following beneficial effects:
[0042] 1) High thermal conductivity: Compared with conventional graphene sheets, the graphene sheets of the present invention can conduct heat more quickly and efficiently.
[0043] 2) Improve toughness: Conventional graphene sheets have poor toughness and are prone to cracks, which affects assembly; however, the thermally conductive graphene sheet of the present invention can effectively improve the toughness problem, increase its bending and assembly reliability, and can better adapt to various stress environments, thereby improving its service life and reliability.
[0044] 3) Low thermal resistance: The surface of conventional graphene sheets is rough, and silicone grease or the like is required to reduce the contact thermal resistance; however, the graphene sheet of the present invention has a smooth and flat surface, so its contact thermal resistance is lower, the resistance encountered during the heat conduction process is smaller, and the heat conduction efficiency is higher.
[0045] 4) Solving the problem of poor vertical thermal conductivity: The thermal conductivity of conventional graphene sheets in the vertical direction is not uniform, resulting in poor overall vertical thermal conductivity. The present invention optimizes the material structure and thermal conduction path to make the graphene sheets have more uniform thermal conductivity in the vertical direction.
[0046] In summary, compared with the prior art, the thermally conductive graphene sheet of the present invention has the advantages of higher thermal conductivity, lower thermal resistance, better toughness and more uniform vertical thermal conductivity.
[0047] Based on the above excellent effects that can be achieved by the technical solution of the present invention, the technical solution of the present invention can be widely used in application fields such as thermal management, electronic device heat dissipation, and new energy. More specifically:
[0048] First, in the field of thermal management, thermally conductive graphene sheets with high thermal conductivity and low thermal resistance can be used to manufacture efficient heat dissipation devices. Nowadays, the integration of various electronic devices continues to increase, resulting in the concentrated release of heat, while the poor toughness and high contact thermal resistance of conventional graphene sheets limit the performance of heat dissipation devices. The thermally conductive graphene sheets prepared using the technical solution of the present invention can effectively improve these problems, provide better thermal conductivity, and thus improve the efficiency and reliability of heat dissipation devices.
[0049] Secondly, in the field of heat dissipation of electronic devices, thermally conductive graphene sheets with high thermal conductivity and low thermal resistance can be used to manufacture high-performance heat sinks, thermally conductive films and other heat dissipation materials. With the continuous increase in the power of electronic devices, the heat dissipation problem has become increasingly prominent. The technical solution of the present invention can effectively improve the thermal conductivity of the thermally conductive graphene sheet, making it an ideal heat dissipation material, which can effectively reduce the temperature of electronic devices and improve their stability and life.
[0050] In addition, in the field of new energy, thermally conductive graphene sheets with high thermal conductivity and low thermal resistance can be applied to photovoltaic cells, electric vehicle batteries and other fields. Photovoltaic cells and electric vehicle batteries generate a lot of heat during operation. If the heat cannot be dissipated in time, it will lead to reduced efficiency and potential safety hazards. The technical solution of the present invention can provide efficient thermal conductivity, help photovoltaic cells and electric vehicle batteries to dissipate heat in time, and improve their energy conversion efficiency and safety.
[0051] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.
[0052] Comparative Example 1
[0053] Step 1: acid-washing graphite powder with a purity of more than 99% to obtain graphene microsheet raw materials with a purity of more than 99%; screening the graphene microsheet raw materials to obtain 60 μm graphene microsheet raw materials.
[0054] Step 2: The obtained graphene microsheet raw material is cleaned and then immersed in a silicone modifier at a temperature of 25°C for about 30 minutes. During the immersion period, the surface of the graphene microsheet is modified by π-π conjugation. After the immersion, the graphene microsheet is screened and dried to obtain modified graphene microsheets with increased toughness and filling properties.
[0055] Step 3: Accurately weigh 80 parts by mass of the modified graphene microsheets and add them to a benzene solvent, ultrasonicate them at room temperature for 10 minutes, stir and disperse them for 30 minutes, and then ultrasonicate and disperse them for 10 minutes to obtain a uniform graphene microsheet slurry.
[0056] Step 4: Accurately weigh 15 parts by mass of organic silica gel water (vinyl-containing polydimethylsiloxane) into the above-mentioned graphene microsheet slurry, ultrasonicate for 10 minutes at room temperature, stir and disperse for 30 minutes, and then ultrasonicate and disperse for 10 minutes to make the organic silica gel water evenly distributed in the entire graphene microsheet slurry to obtain a graphene microsheet rubber.
[0057] Step 5: Using a 20 μm thick glass fiber sheet as a carrier, the prepared graphene microsheet adhesive is scraped onto both sides of the glass fiber, and then baked and dried to obtain a semi-finished product with a thickness of about 400 μm.
[0058] Step 6: The semi-finished product is subjected to hot pressing treatment at 150-160° C. and 10 MPa for 90 seconds to obtain a thermally conductive graphene sheet.
[0059] Example 1
[0060] Step 1: acid-washing graphite powder with a purity of more than 99% to obtain graphene microsheet raw materials with a purity of more than 99%; screening the graphene microsheet raw materials to obtain 60 μm graphene microsheet raw materials.
[0061] Step 2: The obtained graphene microsheet raw material is cleaned and then immersed in a silicone modifier at a temperature of 25°C for about 30 minutes. During the immersion period, the surface of the graphene microsheet is modified by π-π conjugation. After the immersion, the graphene microsheet is screened and dried to obtain modified graphene microsheets with increased toughness and filling properties.
[0062] Step 3: Accurately weigh 80 parts by mass of the modified graphene microsheets and add them to a benzene solvent, ultrasonicate them at room temperature for 10 minutes, stir and disperse them for 30 minutes, and then ultrasonicate and disperse them for 10 minutes to obtain a uniform graphene microsheet slurry.
[0063] Step 4: Accurately weigh 20 parts by mass of boron nitride with a particle size of 60 μm and 15 parts by mass of organic silica gel water (vinyl-containing polydimethylsiloxane) and add them to the above-mentioned graphene microsheet slurry, and ultrasonicate for 10 minutes at room temperature, stir and disperse for 30 minutes, and then ultrasonicate and disperse for 10 minutes to make the boron nitride and organic silica gel water evenly distributed in the entire thermal conductive graphene microsheet slurry to obtain a graphene microsheet slurry.
[0064] Step 5: Using a 20 μm thick glass fiber sheet as a carrier, the prepared graphene microsheet adhesive is scraped onto both sides of the glass fiber, and then baked and dried to obtain a semi-finished product with a thickness of about 400 μm.
[0065] Step 6: The semi-finished product is subjected to hot pressing treatment at 150-160° C. and 10 MPa for 90 seconds to obtain a thermally conductive graphene sheet.
[0066] Example 2
[0067] Step 1: acid-washing graphite powder with a purity of more than 99% to obtain graphene microsheet raw materials with a purity of more than 99%; screening the graphene microsheet raw materials to obtain 60 μm graphene microsheet raw materials.
[0068] Step 2: The obtained graphene microsheet raw material is cleaned and then immersed in a silicone modifier at a temperature of 25°C for about 30 minutes. During the immersion period, the surface of the graphene microsheet is modified by π-π conjugation. After the immersion, the graphene microsheet is screened and dried to obtain modified graphene microsheets with increased toughness and filling properties.
[0069] Step 3: Accurately weigh 80 parts by mass of the modified graphene microsheets and add them to a benzene solvent, ultrasonicate them at room temperature for 10 minutes, stir and disperse them for 30 minutes, and then ultrasonicate and disperse them for 10 minutes to obtain a uniform graphene microsheet slurry.
[0070] Step 4: Accurately weigh 40 parts by mass of boron nitride with a particle size of 60 μm and 15 parts by mass of silicone gel (vinyl-containing polydimethylsiloxane) and add them to the above-mentioned graphene microsheet slurry, and ultrasonicate for 10 minutes at room temperature, stir and disperse for 30 minutes, and then ultrasonicate and disperse for 10 minutes to make the boron nitride and silicone gel evenly distributed in the entire thermal conductive graphene microsheet slurry to obtain a graphene microsheet compound.
[0071] Step 5: Using a 20 μm thick glass fiber sheet as a carrier, the prepared graphene microsheet adhesive is scraped onto both sides of the glass fiber, and then baked and dried to obtain a semi-finished product with a thickness of about 400 μm.
[0072] Step 6: The semi-finished product is subjected to hot pressing treatment at 150-160° C. and 10 MPa for 90 seconds to obtain a thermally conductive graphene sheet.
[0073] Example 3
[0074] Step 1: acid-washing graphite powder with a purity of more than 99% to obtain graphene microsheet raw materials with a purity of more than 99%; screening the graphene microsheet raw materials to obtain 60 μm graphene microsheet raw materials.
[0075] Step 2: The obtained graphene microsheet raw material is cleaned and then immersed in a silicone modifier at a temperature of 25°C for about 30 minutes. During the immersion period, the surface of the graphene microsheet is modified by π-π conjugation. After the immersion, the graphene microsheet is screened and dried to obtain modified graphene microsheets with increased toughness and filling properties.
[0076] Step 3: Accurately weigh 80 parts by mass of the modified graphene microsheets and add them to a benzene solvent, ultrasonicate them at room temperature for 10 minutes, stir and disperse them for 30 minutes, and then ultrasonicate and disperse them for 10 minutes to obtain a uniform graphene microsheet slurry.
[0077] Step 4: Accurately weigh 80 parts by mass of boron nitride with a particle size of 60 μm and 15 parts by mass of organic silica gel water (vinyl-containing polydimethylsiloxane) and add them to the above-mentioned graphene microsheet slurry, and ultrasonicate them at room temperature for 10 minutes, stir and disperse them for 30 minutes, and then ultrasonicate and disperse them for 10 minutes to make the boron nitride and organic silica gel water evenly distributed in the entire thermal conductive graphene microsheet slurry to obtain a graphene microsheet slurry.
[0078] Step 5: Using a 20 μm thick glass fiber sheet as a carrier, the prepared graphene microsheet adhesive is scraped onto both sides of the glass fiber, and then baked and dried to obtain a semi-finished product with a thickness of about 400 μm.
[0079] Step 6: The semi-finished product is subjected to hot pressing treatment at 150-160° C. and 10 MPa for 90 seconds to obtain a thermally conductive graphene sheet.
[0080] Performance Evaluation
[0081] The components of the graphene microplatelet rubber used in the above-mentioned comparative example 1 and embodiments 1 to 3 are summarized in Table 1, and the performance test results of the products are summarized in Table 2.
[0082] Table 1 Graphene microplatelet rubber composition
[0083]
[0084] Table 2 Performance test results
[0085]
[0086] It can be seen from Table 2 that the preparation method adopted in the embodiment of the present invention can improve the problems of poor toughness, high contact thermal resistance and poor vertical thermal conductivity of conventional graphene sheets.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A thermally conductive graphene sheet, characterized in that: The thermal conductive graphene sheet semi-finished product is made by hot pressing. The thermal conductive graphene sheet semi-finished product comprises a glass fiber sheet and a graphene microsheet adhesive layer composited on both sides of the glass fiber sheet. The components of the graphene microsheet adhesive layer include organic silicon surface modified graphene microsheets, boron nitride and organic silica gel water; the thickness of the glass fiber sheet is 10-50 μm, and the thickness of the graphene microsheet adhesive layer on one side of the glass fiber sheet is 50-200 μm; the pressure of the hot pressing is 5-15 MPa, and the temperature of the hot pressing is 140-180°C.
2. The thermally conductive graphene sheet according to claim 1, characterized in that: The particle size of the graphene microsheets in the organic silicon surface-modified graphene microsheets is 30-100 μm.
3. The thermally conductive graphene sheet according to claim 1, characterized in that: The particle size of the boron nitride is 30-100 μm.
4. The thermally conductive graphene sheet according to claim 1, characterized in that: The mass ratio of the organic silicon surface modified graphene microsheets, boron nitride and organic silicon water is 80: (5-30): (20-80).
5. A method for preparing a thermally conductive graphene sheet according to any one of claims 1 to 4, characterized in that: The following steps are involved: a) mixing organic silicon surface modified graphene microsheets, boron nitride, organic silicon water and solvent to obtain graphene microsheet rubber material; b) coating the graphene microsheet sizing material on both sides of the glass fiber sheet and drying the sizing material to obtain a semi-finished thermally conductive graphene sheet; c) hot-pressing the semi-finished thermally conductive graphene sheet to obtain a thermally conductive graphene sheet.
6. The preparation method according to claim 5, characterized in that: In step a), the organosilicon surface-modified graphene microsheets are prepared according to the following steps: soaking the graphene microsheet raw material in an organosilicon modifier, taking out and drying, to obtain the organosilicon surface-modified graphene microsheets.
7. The preparation method according to claim 6, characterized in that: The graphene microsheet raw material is prepared according to the following steps: graphite powder is acid-washed to obtain the graphene microsheet raw material.
8. The preparation method according to claim 5, characterized in that: In step a), the specific process of mixing includes: firstly mixing the organic silicon surface modified graphene microsheets and a solvent to obtain a graphene microsheet slurry; and then mixing the graphene microsheet slurry, boron nitride and organic silicon water to obtain a graphene microsheet slurry.