Method for detecting cracks in passivation layer on chip and method for determining chip yield
By using a heated potassium hydroxide solution to corrode the silicon oxide layer of the chip, and observing the color change of the metal layer with a microscope, the problem of existing technology being unable to detect cracks in the silicon nitride layer but not deep into the silicon oxide layer has been solved, and the chip yield has been improved. Accurate evaluation and efficient detection extend the service life of the chip.
Patent Information
- Application Number
- CN202410670976.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-05-28
AI Technical Summary
Existing chip passivation layer crack detection methods cannot effectively detect cracks in the silicon nitride layer but do not penetrate deep into the silicon oxide layer, resulting in the inability to fully evaluate the chip yield and possibly causing the chip to fail during end use.
The chip is immersed in heated potassium hydroxide solution to corrode the silicon oxide layer, and the color change of the metal layer is observed through a microscope to detect whether there are cracks in the passivation layer. The 35% concentration of the potassium hydroxide solution and the temperature of 90°C are used to maximize the The corrosion rate of the silicon oxide layer ensures the accuracy of crack detection.
It realizes the detection of cracks that penetrate the silicon nitride layer but not the silicon oxide layer, improves the accuracy and detection rate of chip yield assessment, reduces costs, and extends the service life of the chip.
Smart Images

Figure CN118280866B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for detecting cracks in a passivation layer on a chip and a method for determining a chip yield. Background Art
[0002] In order to protect the chip from external environmental moisture, ion pollution, chemical hazards and mechanical stress, a layer of silicon nitride and silicon oxide film is deposited on the chip surface as a passivation layer. At the same time, the internal stress of the passivation layer is very sensitive to changes in the external environmental temperature. Therefore, there is a risk of cracking in the passivation layer, and the cracked passivation layer loses its protective effect on the chip.
[0003] In order to detect the cracking of the passivation layer, the current method is to immerse the metal in a 40°C 85% phosphoric acid (H3PO4) solution. The main principle of this method is that phosphoric acid hardly reacts with silicon nitride and silicon oxide at 40°C, that is, the reaction rate is about 0nm / min. Therefore, phosphoric acid can enter the metal aluminum (Al) in the lower layer through the cracks of the passivation layer without destroying the structure of the passivation layer to carry out a chemical reaction. The reaction equation is: 2Al+6H3PO4==2Al(H2PO4)3+3H2↑. Since the dihydrogen phosphate (Al(H2PO4)3) generated by the reaction is easily soluble in water, the reaction will corrode the metal aluminum into a cavity. In this way, the reaction area has a color difference with the unreacted metal next to it under an optical microscope (OM), so the cracks in the passivation layer can be detected by color. Figure 1 The left picture shows an image observed under an optical display microscope in the above detection method. The lower left corner of the through hole framed by the dotted line has a color difference with the surrounding metal. This area is the area where the reaction occurs, indicating that a crack in the passivation layer has been detected. The arrow points to Figure 1 The passivation layer crack in the middle right picture is the passivation layer crack detected here.
[0004] However, the above method can only detect the phenomenon that the passivation layer breaks to the metal layer. Figure 2 The cracks outlined by the dashed lines do not penetrate into the silicon oxide) or the silicon nitride is broken but the silicon oxide is not completely broken (such as Figure 3 The cracks outlined by the dotted lines penetrate into the silicon oxide but do not penetrate the silicon oxide), and phosphoric acid cannot enter the metal layer below the passivation layer. In this way, the above method cannot detect the defect of the passivation layer rupture, and the chip is likely to fail in terminal use. Summary of the invention
[0005] In view of the above problems, the present application provides a method for detecting cracks in a passivation layer on a chip, aiming to detect defects in which cracks in the passivation layer penetrate the silicon nitride layer but do not penetrate the silicon oxide layer.
[0006] According to a first aspect of the present invention, a method for detecting cracks in a passivation layer on a chip is provided, wherein the passivation layer comprises a silicon nitride layer and a silicon oxide layer in contact with the silicon nitride layer, and the silicon oxide layer also contacts a metal layer of the chip, and the detection method comprises:
[0007] Immersing the chip in a heated potassium hydroxide solution so that the heated potassium hydroxide solution corrodes the silicon oxide layer while passing through the silicon nitride layer and enters the metal layer;
[0008] The chip is placed under a microscope to observe the color of the metal layer to determine whether there are cracks in the passivation layer.
[0009] Optionally, the concentration of the potassium hydroxide solution is configured to be 35%.
[0010] Optionally, the temperature of the heated potassium hydroxide solution is 90°C.
[0011] Optionally, the time for which the chip is immersed in the heated potassium hydroxide solution is determined according to the maximum value of the distance from different positions on the contact surface of the silicon nitride layer and the silicon oxide layer to the metal layer and the corrosion rate of the silicon oxide layer by the heated potassium hydroxide solution.
[0012] Optionally, after immersing the chip in a heated potassium hydroxide solution and before placing the chip under a microscope to observe the color of the metal layer to determine whether the passivation layer has cracks, the detection method further includes: cleaning the chip with deionized water.
[0013] Optionally, before immersing the chip in the heated potassium hydroxide solution, the detection method further comprises:
[0014] Immersing the chip in a potassium hydroxide solution so that the potassium hydroxide solution enters the metal layer while passing through the passivation layer;
[0015] The chip is placed under a microscope to observe the color of the metal layer to determine whether there are cracks penetrating the passivation layer.
[0016] Optionally, the detection method also includes: when it is determined that there are cracks in the passivation layer that penetrate the passivation layer, recording the corresponding areas in the metal layer where there are color differences, so as to determine whether there are cracks in the passivation layer that penetrate the silicon nitride layer but not the silicon oxide layer based on the recorded areas when it is determined that there are cracks in the passivation layer.
[0017] Optionally, after immersing the chip in a potassium hydroxide solution and before placing the chip under a microscope to observe the color of the metal layer to determine whether there are cracks in the passivation layer that penetrate the passivation layer, the detection method further includes: cleaning the chip with deionized water.
[0018] Optionally, the chip is immersed in a potassium hydroxide solution with the surface intact.
[0019] According to a second aspect of the present invention, a method for determining chip yield is provided, comprising: using any one of the detection methods described in the first aspect to determine whether there are passivation layer cracks in each of a plurality of chips to be detected, and determining the chip yield based on the detection results of each of the plurality of chips.
[0020] The unexpected technical effects of this application are:
[0021] According to the detection method of the embodiment of the present invention, the chip is immersed in a heated potassium hydroxide solution, and then the chip is placed under a microscope to observe the color of the metal layer to determine whether there are cracks in the passivation layer. Since the heated potassium hydroxide solution can corrode silicon oxide but cannot corrode silicon nitride, as long as the cracks in the passivation layer penetrate the silicon nitride layer, the heated potassium hydroxide solution can corrode the silicon oxide layer and enter the metal layer to react with the metal layer, so that the cracks can be detected, including cracks that penetrate the entire passivation layer and cracks that penetrate the silicon nitride layer but not the silicon oxide layer.
[0022] Furthermore, the concentration of the potassium hydroxide solution is configured to be 35%. This is because it has been experimentally determined that at temperatures where the corrosion rate of the silicon oxide layer meets the conventional requirements of existing chips, the corrosion rate of the silicon oxide by the potassium hydroxide solution at a concentration of 35% is the greatest among the multiple concentrations, which is conducive to achieving a higher detection rate at a lower cost.
[0023] Furthermore, before immersing the chip in the heated potassium hydroxide solution, the chip can be immersed in the potassium hydroxide solution first and then the chip can be placed under a microscope to observe the color of the metal layer to determine whether there are cracks in the passivation layer that penetrate the passivation layer. In this way, when the chip is subsequently placed under a microscope to observe the color of the metal layer and it is determined that there are cracks in the passivation layer, it can be more specifically determined based on the detection results here whether there are cracks in the passivation layer that penetrate the silicon nitride layer but not the silicon oxide layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The above and other objects, features and advantages of the present application will become more apparent through the following description of the embodiments of the present application with reference to the accompanying drawings, in which:
[0025] Figure 1 Shown is a schematic diagram of detecting cracks in the passivation layer using an existing detection method;
[0026] Figure 2 An exemplary crack that does not penetrate the passivation layer is shown;
[0027] Figure 3 Another exemplary crack that does not penetrate the passivation layer is shown;
[0028] Figure 4 Shown is a schematic cross-sectional view of a chip;
[0029] Figure 5 Shown is a flow chart of a method for detecting cracks in a passivation layer on a chip provided by an embodiment of the present application;
[0030] Figure 6 Shown are the corrosion rate curves of silicon oxide at different temperatures of potassium hydroxide solutions of nine concentrations respectively obtained through experimental fitting in the embodiments of the present application;
[0031] Figure 7 Shown is a cross-sectional view of an exemplary chip;
[0032] Figure 8 Shown is a flow chart of another method for detecting cracks in a passivation layer on a chip provided by an embodiment of the present application;
[0033] Fig. 9 Shown Figure 4 The corrosion condition of the chip shown after being immersed in a potassium hydroxide solution according to the detection method provided in the embodiment of the present application;
[0034] Fig.10 Shown Fig. 9 The corrosion condition of the chip shown after being immersed in a heated potassium hydroxide solution according to the detection method provided in the embodiment of the present application;
[0035] FIG. 11 ( a ) shows an image of an exemplary chip under an optical microscope before being immersed in a potassium hydroxide solution according to the detection method provided in an embodiment of the present application;
[0036] FIG11( b ) is an image of the chip shown in FIG11( a ) under an optical microscope after being immersed in a potassium hydroxide solution at room temperature according to the detection method provided in an embodiment of the present application;
[0037] FIG11( c ) is an image of the chip shown in FIG11( b ) under an optical microscope after being immersed in a heated potassium hydroxide solution according to the detection method provided in an embodiment of the present application;
[0038] Fig.12 Shown is a flow chart of a method for determining chip yield provided by another embodiment of the present application. DETAILED DESCRIPTION
[0039] The present application will be described in more detail below with reference to the accompanying drawings. In each of the accompanying drawings, the same elements are represented by similar reference numerals. For the sake of clarity, the various parts in the accompanying drawings are not drawn to scale. In addition, some well-known parts may not be shown. The present application can be presented in various forms, some examples of which will be described below.
[0040] This application may be presented in a variety of forms, some examples of which are described below.
[0041] Figure 4 A schematic cross-sectional view of a chip is shown. The chip is, for example, a semiconductor device MOSFET (Metal-Oxide-Semiconductor Field-Effect Transistor), but is not limited thereto. In a preferred embodiment, the chip is, for example, an N-type MOSFET. Figure 4 As shown, the chip 100 includes a semiconductor layer 110 , an interlayer dielectric layer 120 formed on the semiconductor layer 110 , a metal layer 130 formed on the interlayer dielectric layer 120 , and a passivation layer 140 formed on the metal layer 130 .
[0042] The semiconductor layer 110 may be composed of any one selected from a doped semiconductor substrate, a doped well region, and a doped epitaxial semiconductor layer. For example, for an N-type MOSFET, the semiconductor layer 110 is P-type doped; for a P-type MOSFET, the semiconductor layer 110 is N-type doped. A source region and a drain region may be formed in the semiconductor layer 110. The source region and the drain region are doped regions in the semiconductor layer 110. For example, for an N-type MOSFET, the source region and the drain region are N-type doped; for a P-type MOSFET, the source region and the drain region are P-type doped. A shallow trench structure may also be formed in the semiconductor layer 110. The shallow trench structure is used to separate adjacent semiconductor devices and may be composed of any one selected from silicon oxide, silicon nitride, and silicon oxynitride.
[0043] The interlayer dielectric layer 120 is used to isolate the active area of the chip 100 from the metal layer 130, and is composed of, for example, silicon oxide. A gate dielectric layer and a gate conductor may be formed in the interlayer dielectric layer 120, wherein the gate dielectric layer is sandwiched between the semiconductor layer 110 and the gate conductor, the gate dielectric layer is composed of, for example, silicon oxide, and the gate conductor is composed of, for example, doped polysilicon. Connection holes may also be formed in the interlayer dielectric layer 120, and metal may be filled in the connection holes to form connection channels, and the connection channels are used to connect the above-mentioned source region, drain region, and gate conductor to the metal layer 130. The metal layer 130 is usually formed into a plurality of wirings through an etching process, and the wirings in the metal layer 130 are specifically connected to the above-mentioned connection channels.
[0044] The passivation layer 140 covers the metal layer 130 to protect the metal layer 130. In addition, since the metal layer 130 is usually embodied as a plurality of spaced wirings, part of the surface of the interlayer dielectric layer 120 is exposed between the wirings of the metal layer 130, and thus the passivation layer 140 also covers the interlayer dielectric layer 120, thereby playing a role in protecting the device structures in the interlayer dielectric layer 120. In the process of forming the passivation layer 140, a layer of silicon oxide is usually deposited first and then a layer of silicon nitride is deposited, so the passivation layer 140 includes a silicon oxide layer 141 and a silicon nitride layer 142 in contact with the silicon oxide layer 141, and the silicon oxide layer 141 in contact with the metal layer 130 in the passivation layer 140. Since the film stress in the passivation layer 140 is very sensitive to changes in the external ambient temperature, the passivation layer 140 is at risk of cracking, such as forming a crack 151 that breaks into the metal layer 130 and penetrates the passivation layer 140, and cracks 152 and 153 that do not break into the metal layer 130, wherein the crack 152 only penetrates the silicon nitride layer 142 and does not penetrate into the silicon oxide layer 141, and the crack 153 penetrates the silicon nitride layer 142 and penetrates into the silicon oxide layer 141 but does not penetrate the silicon oxide layer 141, so both cracks 152 and 153 are cracks that penetrate the silicon nitride layer 142 but do not penetrate the silicon oxide layer 141.
[0045] Cracks in the passivation layer 140 may cause moisture, ion pollution, etc. in the external environment to damage the chip 100, causing the chip 100 to fail when used in the terminal. Therefore, after a batch of chips 100 is produced, it is necessary to detect whether there are cracks in the passivation layer 140 to determine the yield of the batch of chips 100 and then determine whether the production process of the batch of chips 100 is reliable. Only when the yield of the batch of chips 100 meets the requirements will it be applied to the terminal.
[0046] Since the cracks in the passivation layer 140 are very fine, they cannot be directly observed with the naked eye or with the aid of a microscope. Figure 4The crack 151 penetrating the passivation layer 140 shown will be detected by immersing in a phosphoric acid solution with a concentration of 85% at 40°C. Specifically, the chip 100 is immersed in a phosphoric acid solution with a concentration of 85% at 40°C, and the phosphoric acid solution enters the metal layer 130 through the crack 151 penetrating the passivation layer 140 to react with the aluminum in the metal layer 130; then the chip 100 is placed under an optical microscope to observe the color of the metal layer 130. Since visible light can pass through the passivation layer 400, the metal layer 130 can be directly observed under an optical microscope, and since the reacted area has a color difference from the unreacted metal next to it under an optical microscope, for example, the reacted area appears blue under an optical microscope while the surrounding unreacted metal appears gold, it can be determined whether the passivation layer 140 has a crack 151 penetrating the passivation layer 140 by observing the color of the metal layer 130. It should be noted that the color of the reacted area in the metal layer 130 under an optical microscope varies depending on the thickness of the passivation layer 140, and the color of the unreacted metal in the metal layer 130 under an optical microscope also varies depending on the thickness of the passivation layer 140. Therefore, when observing the color of the metal layer 130, it is mainly necessary to observe whether there is an area in the metal layer 130 whose color is different from that of the surrounding metal. If so, it is determined that the area is caused by the crack 151 that penetrates the passivation layer 140. Otherwise, it is determined that there is no crack that penetrates the passivation layer 140.
[0047] However, for the cracks 152 and 153 that penetrate the silicon nitride layer 142 but not the silicon oxide layer 141, since the phosphoric acid solution hardly reacts with silicon nitride and silicon oxide, the phosphoric acid solution cannot reach the metal layer 130, so the phosphoric acid solution cannot react with the aluminum in the metal layer 130, resulting in detection failure.
[0048] In order to detect cracks in the passivation layer 140 that penetrate the silicon nitride layer 142 but do not penetrate the silicon oxide layer 141, an embodiment of the present application provides a method for detecting cracks in the passivation layer on a chip. The detection method is implemented using a potassium hydroxide (KOH) solution and is mainly used to detect cracks in the passivation layer 140 of a chip 100 whose metal layer 130 is made of aluminum or aluminum alloy. Figure 5 FIG. 1 is a flow chart of a method for detecting cracks in a passivation layer provided in an embodiment of the present application. Figure 5 As shown, the detection method includes:
[0049] Step S120, immersing the chip 100 in a heated potassium hydroxide solution, so that the heated potassium hydroxide solution corrodes the silicon oxide layer 141 while passing through the silicon nitride layer 142 and enters the metal layer 130;
[0050] Step S140 , placing the chip 100 under a microscope to observe the color of the metal layer 130 to determine whether there are cracks in the passivation layer 140 .
[0051] Specifically, silicon nitride hardly reacts in potassium hydroxide solution, regardless of whether it is heated or not; silicon oxide reacts violently in heated potassium hydroxide solution, and the reaction equation is: SiO2+ 2KOH == K2SiO3+ H2O, and it does not react without heating; potassium hydroxide solution and aluminum also react violently, and the reaction equation is: 2Al+2KOH+2H2O==2KAlO2+3H2↑. Therefore, during the execution of step S120, if there are cracks in the passivation layer 140 and the existing cracks penetrate the silicon nitride layer 142, then in this case, the heated potassium hydroxide solution will pass through the silicon nitride layer 142 and then corrode the silicon oxide layer 141 to enter the metal layer 130 and react with the aluminum in the metal layer 130, and after the reaction, potassium silicate (K2SiO3) and potassium aluminate (KAlO2) that are easily soluble in water will be generated; then during the execution of step S140, it can be observed that there are areas in the metal layer 130 that are different in color from the surrounding metal, thereby determining that there are cracks in the passivation layer 140.
[0052] It should be noted that the above detection method can detect cracks as long as they penetrate the silicon nitride layer 142, including Figure 4 The crack 151 that penetrates the passivation layer 140 and the cracks 152 and 153 that penetrate the silicon nitride layer 142 but not the silicon oxide layer 141 are shown in the figure. Therefore, they are of great significance in reducing the frequency of chip failure during terminal use, which is beneficial to promoting the service life of chips in various products on the market.
[0053] Figure 6 The figure shows the corrosion rate curves of silicon oxide at different temperatures for nine concentrations of potassium hydroxide solution fitted by experiments. The nine concentrations are 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% and 60%. Figure 6 As shown, at a temperature where the corrosion rate of at least one concentration of potassium hydroxide solution on silicon oxide is greater than 500nm / h (about 8.3nm / min), the 35% concentration of potassium hydroxide solution among the nine concentrations has the highest corrosion rate on silicon oxide. Therefore, in some examples, the concentration of the potassium hydroxide solution in step S120 is configured to be 35%. In this way, the potassium hydroxide used for detection is as small as possible, but the corrosion rate of the silicon oxide layer 141 is as large as possible while the corrosion rate of the silicon oxide layer 141 meets the conventional requirements of existing chips, which is conducive to achieving a higher detection rate at a lower cost. Further, the temperature of the heated potassium hydroxide solution in step S120 is controlled at 90°C, as shown in FIG. Figure 6 As shown, the corrosion rate of the silicon oxide layer 141 by the potassium hydroxide solution with a concentration of 35% at this temperature is 0.98um / h, so the corrosion depth of 10nm takes about half a minute. For the existing nano-scale process chips, the corrosion time is neither too long nor too short to be uncontrollable.
[0054] Furthermore, the time T for which the chip 100 is immersed in the heated potassium hydroxide solution in step S120 is determined based on the maximum value Lmax of the distance from different positions on the contact surface of the silicon nitride layer 142 and the silicon oxide layer 141 to the metal layer 130 and the corrosion rate V of the heated potassium hydroxide solution on the silicon oxide layer 141. The quotient obtained by dividing the maximum value Lmax by the corrosion rate V can be determined as the time T; or a time slightly larger than the above-mentioned quotient can be determined as the time T. This is to accurately ensure that the heated potassium hydroxide solution can enter the metal layer 130 after corroding the silicon oxide layer 141 after passing through the silicon nitride layer 142, so as to prevent the heated potassium hydroxide solution from being unable to enter the metal layer 130 after passing through the silicon nitride layer 142 due to incomplete corrosion of the silicon oxide layer 141.
[0055] It should be noted that there are multiple paths from any position on the contact surface of the silicon nitride layer 142 and the silicon oxide layer 141 to the metal layer 130, among which the shortest straight line path is the distance from the position to the metal layer 130. The distance from the position to the metal layer 130 is also referred to as the thickness of the silicon oxide layer 141 on the metal layer 130 at the position in the embodiment of the present application. Therefore, the above-mentioned maximum value Lmax can also be understood as the maximum thickness of the silicon oxide layer 141 on the metal layer 130.
[0056] Figure 7 A cross-sectional view of an exemplary chip is shown. Figure 7 , double arrows 1 and 2 indicate the thickness of the silicon nitride layer 142 at two different positions, double arrows 3 and 4 indicate the thickness of the silicon nitride layer 141 on the metal layer 130 at two different positions, wherein the thickness indicated by double arrow 4 is the maximum value Lmax of the distance from different positions on the contact surface of the silicon nitride layer 142 and the silicon oxide layer 141 to the metal layer 130 and is 0.43um. If a potassium hydroxide solution with a concentration of 35% at 90°C is used to etch the silicon oxide layer 141 during the test, the time T for the chip 100 to be immersed in the heated potassium hydroxide solution in step S120 can be the time obtained by dividing 0.43um by 0.98um / h.
[0057] Furthermore, the detection method provided in the embodiment of the present application also includes, after executing step S120 and before executing step S140, washing the chip 100 with deionized water to remove possible ions, including ions in the unreacted potassium hydroxide solution or ions in potassium silicate and potassium aluminate generated by the reaction, so as to avoid damage to the instrument used in step S140 by the alkaline solution or the acidic solution. It should be understood that if there is liquid attached to the chip 100 after washing with deionized water, it needs to be dried, and a hair dryer or other equipment can be used to dry it in order to improve the detection efficiency.
[0058] Figure 8 FIG. 1 is a flow chart of another method for detecting cracks in a passivation layer provided in an embodiment of the present application. Figure 8 As shown, the detection method includes:
[0059] Step S112, immersing the chip 100 in a potassium hydroxide solution, so that the potassium hydroxide solution enters the metal layer 130 while passing through the passivation layer 140;
[0060] Step S114 , placing the chip 100 under a microscope to observe the color of the metal layer 130 to determine whether there are cracks penetrating the passivation layer 140 .
[0061] Step S120, immersing the chip 100 in a heated potassium hydroxide solution, so that the heated potassium hydroxide solution corrodes the silicon oxide layer 141 while passing through the silicon nitride layer 142 and enters the metal layer 130;
[0062] Step S140 , placing the chip 100 under a microscope to observe the color of the metal layer 130 to determine whether there are cracks in the passivation layer 140 .
[0063] Fig. 9 Shown Figure 4 The chip 100 shown in FIG. 1 is corroded after step S112 is performed. Fig. 9 As shown, since the potassium hydroxide solution does not react with silicon nitride and silicon oxide without heating, the potassium hydroxide solution can only enter the metal layer 130 through the crack 151 that penetrates the passivation layer 140 and react with the aluminum in the wiring below the crack 151 in the metal layer 130 to form a cavity 161. During the execution of step S114, it can be observed that the location of the cavity 161 in the metal layer 130 has a color difference with the surrounding metal, thereby determining that there is a crack 151 that penetrates the passivation layer 140.
[0064] Fig.10 Shown Fig. 9 The corrosion condition of the chip 100 after step S120 is performed is shown. Fig.10 As shown, since the heated potassium hydroxide solution does not react with silicon nitride but reacts with silicon oxide and aluminum, not only will the void 161 expand, but the heated potassium hydroxide solution will enter the metal layer 130 through the cracks 152 and 153 and then corrode the silicon oxide layer 141, and react with the aluminum in the wiring below the cracks 152 and 153 in the metal layer 130 to form voids 162 and 163. Afterwards, during the execution of step S140, it can be observed that the positions of the voids 161, 162 and 163 in the metal layer 130 are different in color from the surrounding metal, thereby confirming the presence of cracks 151, 152 and 153 that penetrate the passivation layer 140.
[0065] Specifically, the microscope used in the above step S114 and step S140 is, for example, an optical microscope.
[0066] It should be noted that, since the reaction speed between potassium hydroxide solution and aluminum is relatively fast, the time for the chip 100 to be immersed in the potassium hydroxide solution in step S112 is in the order of seconds, for example, 30 seconds.
[0067] Further, in this embodiment, if it is determined that there is a crack that penetrates the passivation layer 140 after step S112 is executed, the corresponding area in the metal layer 130 where the color is different can be recorded. In this way, if it is determined that there is a crack in the passivation layer 140 after step S140 is executed, it can be determined whether there is a crack in the passivation layer 140 that penetrates the silicon nitride layer 142 but does not penetrate the silicon oxide layer 141 based on the recorded area. Fig. 9 In the example shown, the area where the hole 161 is located is recorded, and then Fig.10 In the case where the positions of the holes 161, 162 and 163 shown are different in color from the surrounding metal, it can be determined that the positions of the holes 162 and 163 are different in color from the surrounding metal due to the presence of cracks 152 and 153 that penetrate the silicon nitride layer 142 but not the silicon oxide layer 141. This detection result of more detailed determination of the type of crack after determining that the passivation layer 140 has cracks is conducive to subsequent targeted improvements to the production process of the chip 100.
[0068] FIG11(a) shows an image of an exemplary chip under an optical microscope before being immersed in a potassium hydroxide solution, FIG11(b) shows an image of the chip shown in FIG11(a) under an optical microscope after being immersed in a potassium hydroxide solution at room temperature, and FIG11(c) shows an image of the chip shown in FIG11(b) under an optical microscope after being further immersed in a heated potassium hydroxide solution. Referring to these three images, it can be seen that FIG11(b) adds a void Q1 with a color different from the surrounding metal compared to FIG11(a), and FIG11(c) adds voids Q2 and Q3 with a color different from the surrounding metal compared to FIG11(b), wherein void Q1 is caused by a crack that penetrates the passivation layer on the chip, and voids Q2 and Q3 are caused by cracks that penetrate the silicon nitride layer but not the silicon oxide layer on the chip.
[0069] Furthermore, the detection method provided in the embodiment of the present application further includes, after executing step S112 and before executing step S114, washing the chip 100 with deionized water to wash away possible ions, thereby preventing the alkaline solution or the acidic solution from damaging the instrument used in step S114. It should be understood that if there is liquid attached to the chip 100 after washing with deionized water, it needs to be dried, and a hair dryer or other equipment can be used to dry it in order to improve the detection efficiency.
[0070] The detection method provided in the embodiment of the present disclosure is mainly for detecting the yield of the chip. Therefore, before executing step S112, it is possible to first check whether the chip surface is intact. If there are obvious defects such as scratches and edge collapse, the chip does not need to be detected by the detection method provided in this application. If the surface is intact, the chip 100 in step S112 is immersed in the potassium hydroxide solution.
[0071] In some cases, the chip 100 uses aluminum pins, so the aluminum pins will also be corroded after the above detection method is executed. It should be understood that the color of the metal layer 130 observed under the microscope does not take the color change of the aluminum pins into account.
[0072] Corresponding to the detection method of passivation layer cracks on a chip provided in the above embodiments, another embodiment of the present application also provides a method for determining chip yield, which includes: using any of the detection methods for passivation layer cracks on a chip provided in the above embodiments to determine whether there are passivation layer cracks in each of the multiple chips to be tested, and determining the chip yield based on the detection results of each of the multiple chips.
[0073] Fig.12 FIG. 1 is a flow chart of a method for determining chip yield provided by an embodiment of the present application. Fig.12 As shown, the determination method includes:
[0074] Step S210, for each chip among the plurality of chips to be tested, immersing the chip in a heated potassium hydroxide solution and then observing the chip under a microscope to test whether there are cracks in the passivation layer thereof;
[0075] Step S220, determining the chip yield rate according to the detection results of each of the multiple chips.
[0076] Specifically, during the execution of the determination method, a batch of chips produced by a production process can be selected, and then the chips with incomplete surfaces among the selected chips can be recorded as bad chips, and the chips with intact surfaces can be used as multiple chips to be tested for passivation layer crack detection. If the detection result of any chip among the multiple chips shows that there is a passivation layer crack, it is determined to be a bad chip, and the yield of the batch of chips is obtained by subtracting the ratio of the total number of all bad chips to the total number of chips in the whole batch from 1.
[0077] It should be noted that Fig.12 In the determination method shown, step S210 is a detection method for cracks in the passivation layer on a chip provided in the above embodiment, and other detection methods provided in the above embodiment may also be used in other examples. In addition, after the execution of step S210, the aluminum pins of the chip will be corroded and no longer used, so step S210 belongs to destructive detection, so the determination method provided in the embodiment of the present application is only to determine the chip yield and then determine whether the production process of the chip is reliable.
[0078] The chip yield determination method provided in the example of the present application is more reliable because the detection result of the passivation layer cracks is more accurate.
[0079] The embodiments of the present application are described above, and these embodiments do not describe all the details in detail, nor do they limit the application to the specific embodiments described. Obviously, many modifications and changes can be made based on the above description. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present application, so that those skilled in the art can make good use of the present application and the modifications based on the present application. The present application is only limited by the claims and their full scope and equivalents.
Claims
1. A method for detecting cracks in a passivation layer on a chip, wherein the passivation layer comprises a silicon nitride layer and a silicon oxide layer in contact with the silicon nitride layer, and the silicon oxide layer also contacts a metal layer of the chip, the detection method comprising: Immersing the chip in a potassium hydroxide solution, so that the potassium hydroxide solution enters the metal layer through cracks penetrating the passivation layer in a manner that does not react with the passivation layer to corrode the metal layer; Placing the chip under a microscope and observing the color of the metal layer to determine whether there is a crack in the passivation layer that penetrates the passivation layer; Immersing the chip in a heated potassium hydroxide solution, so that the heated potassium hydroxide solution corrodes the silicon oxide layer while passing through the silicon nitride layer and enters the metal layer to corrode the metal layer; The chip is placed under a microscope to observe the color of the metal layer to determine whether there are cracks in the passivation layer.
2. The detection method according to claim 1, wherein: The concentration of potassium hydroxide solution was prepared to be 35%.
3. The detection method according to claim 2, wherein: The temperature of the heated potassium hydroxide solution was 90°C.
4. The detection method according to claim 1, wherein: The time period for which the chip is immersed in the heated potassium hydroxide solution is determined according to the maximum value of the distance from different positions on the contact surface of the silicon nitride layer and the silicon oxide layer to the metal layer and the corrosion rate of the heated potassium hydroxide solution on the silicon oxide layer.
5. The detection method according to claim 1, after immersing the chip in a heated potassium hydroxide solution and before placing the chip under a microscope to observe the color of the metal layer to determine whether the passivation layer has cracks, further comprising: The chip was cleaned by deionized water.
6. The detection method according to claim 1, further comprising: When it is determined that cracks exist in the passivation layer, the corresponding areas in the metal layer where there are color differences are recorded, so as to determine whether cracks exist in the passivation layer that penetrate the silicon nitride layer but not the silicon oxide layer based on the recorded areas.
7. The detection method according to claim 1, after immersing the chip in a potassium hydroxide solution and before placing the chip under a microscope to observe the color of the metal layer to determine whether there are cracks in the passivation layer that penetrate the passivation layer, further comprising: The chip was cleaned by deionized water.
8. The detection method according to claim 1, wherein: The chip was immersed in a potassium hydroxide solution with the surface intact.
9. A method for determining chip yield, comprising: The detection method described in any one of claims 1 to 8 is used to determine whether each of the multiple chips to be detected has a passivation layer crack, and the chip yield is determined based on the detection results of each of the multiple chips.