A super hydrophilic softener emulsion and preparation method thereof
Through the polymerization of γ-aminopropyltriethoxysilane, tetrakis (hydroxyethyl) silane and octamethylcyclotetrasiloxane and the use of polyether modifiers, a super hydrophilic softener emulsion is formed to solve the current problem. There is a problem in the technology that it is difficult to balance the hydrophilicity and softness of fabrics, and the high hydrophilicity and softness of the fabric is achieved, and the stability of use is improved.
Patent Information
- Application Number
- CN202410720425.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-05
AI Technical Summary
It is difficult for existing softener emulsions to have both hydrophilicity and softness of fabrics at the same time, and there are defects such as yellowing, oil drift, or roller sticking during use.
γ-aminopropyltriethoxysilane, tetrakis (hydroxyethyl) silane and octamethylcyclotetrasiloxane are polymerized to form a polymer compound. By controlling the molar mass ratio and introducing polyether modifiers, a superphilic The water softener emulsion forms a film on the surface of the fabric, improves hydrophilicity and softness, and enhances the water-absorbing properties of the fabric through chemical reactions.
It achieves the excellent softness and resilience of the fabric, while improving the hydrophilic performance, avoiding yellowing and stability problems, and providing better wearing comfort and use stability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile auxiliaries, and particularly relates to a super hydrophilic softener emulsion and a preparation method thereof. Background Art
[0002] Amino silicone oil is widely used in the softening finishing of various natural and synthetic fibers due to its "super soft" fabric finishing effect. The finished fabrics have the advantages of softness, smoothness, good resilience and wrinkle resistance. However, there are also defects such as the hydrophobicity of the fabric making it less comfortable to wear, yellowing of light-colored fabrics after high-temperature baking or ultraviolet irradiation, and poor emulsion stability making it easy to float oil or stick to rollers during use. Therefore, improving the hydrophilicity of amino silicone oil has become a research hotspot.
[0003] At present, the hydrophilic silicone oil finishing agent on the market mainly adopts polyether modified silicone oil finishing agent. Due to the introduction of polyether hydrophilic groups in the molecular structure, the molecular structure contains -CH2CHO groups, which form a zigzag shape in aqueous solution, and the oxygen atoms with high electronegativity are placed on the outside of the main chain, which are easy to combine with hydrogen bonds in water, thereby improving hydrophilicity. The hydrophilicity of the fabric after finishing is greatly improved. However, due to the large amount of polyether hydrophilic groups introduced into the main chain, the polysiloxane is reduced, so the softness of the finished fabric is poor, and it is difficult to achieve the effect of both softness and hydrophilicity. In addition, the whiteness is poor and the yellowing is large.
[0004] The Chinese patent application with publication number CN106498751A discloses a hydrophilic fabric softener, which is made of the following components by weight: 20-30 parts of hydrophilic amino silicone oil, 12-0 parts of dodecylbenzene sulfonic acid, 15-36 parts of fatty alcohol polyoxyethylene ether, 14-25 parts of amino-modified polysiloxane, 21-32 parts of sodium tripolyphosphate, 5-18 parts of hydroxymethyl cellulose, 3-9 parts of acrylamide and 100-150 parts of water. The hydrophilic fabric softener has a smooth hand feel, good bulkiness, improved tearing and friction resistance, but poor hydrophilicity. The Chinese patent application with publication number CN110656500A discloses a non-silicon hydrophilic softener and its preparation method and application, wherein stearic acid, N-methyl diolamine and ester catalyst are mixed to obtain an initial product; polyether diol is added to the initial product to generate a polymer; a quaternary ammonium agent is added to the polymer to obtain the non-silicon hydrophilic softener. The non-silicon hydrophilic softener prepared by this method can effectively improve the hydrophilicity of the textile when used for textile finishing, but its softness is not greatly improved. Summary of the invention
[0005] In order to solve the technical problem that the softener emulsion in the related art cannot have both hydrophilicity and softness, the object of the present invention is to provide a super hydrophilic softener emulsion and a preparation method thereof.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] A method for preparing a super hydrophilic softener emulsion comprises the following steps:
[0008] S1. γ-aminopropyltriethoxysilane and tetra(hydroxyethyl)silane were added to water respectively, stirred and hydrolyzed, and then added to the reaction kettle, nitrogen was introduced, octamethylcyclotetrasiloxane was added, the temperature was raised to 80-85°C, a catalyst was added, the temperature was continued to be raised to 140-145°C, the temperature was kept for 2-3h, unreacted monomers were removed by vacuum, and the amino silicone oil was obtained;
[0009] S2. Add an emulsifier to the amino silicone oil obtained in step S1, stir evenly and heat to 80-90°C, add a modifier dropwise while stirring, keep the reaction warm for 4-5h after the addition is complete, and cool to 25-30°C to obtain a modified amino silicone oil;
[0010] S3. Add an organic acid to the modified amino silicone oil obtained in step S2 to adjust the pH value to 6-7.
[0011] The present invention uses γ-aminopropyl triethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane to polymerize to form the main chain of a polymer compound, which can form a film on the surface of the fabric. The amino group of the high surface energy group in the molecular structure retracts inside the fiber and reacts chemically with the epoxy group, carboxyl group or hydroxyl group on the surface of the fabric, so that the super-hydrophilic softener emulsion is tightly combined with the fabric, and the low surface energy methylsiloxane chain occupies the fiber surface, making the fabric soft and smooth, and giving the fabric excellent softness and resilience. At the same time, the amino group contained in γ-aminopropyl triethoxysilane and the hydroxyl group contained in tetra(hydroxyethyl)silane can be used as a water-absorbing group on the surface of the softener film layer, thereby improving the hydrophilicity of the softener emulsion.
[0012] In addition, the present invention also uses a polyether modifier to modify the prepared amino silicone oil, thereby further improving the hydrophilicity of the super hydrophilic softener emulsion. Since the polyether group is introduced into the amino group of the amino silicone oil, the number of active hydrogen on the amino group can be reduced, thereby increasing the stability of the super hydrophilic softener emulsion.
[0013] Furthermore, in step S1 of the method for preparing the super hydrophilic softener emulsion, the molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane is 13-15:6-10:21-24.
[0014] The present invention controls the number of amino groups, hydroxyl groups and methylsiloxane chains in the molecular structure of the modified amino silicone oil by controlling the molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane, thereby further controlling the softness and hydrophilicity of the obtained super-hydrophilic softener emulsion after film formation. Studies have found that when the molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane exceeds the range provided by the present invention, the obtained super-hydrophilic softener emulsion will make the fabric yellow or the hydrophilicity and softness deteriorate after film formation, which indicates that the number of amino groups or hydroxyl groups is too small and the number of methylsiloxane chains is too large, which will cause the hydrophilicity of the softener emulsion to deteriorate after film formation; the number of amino groups or hydroxyl groups is too large and the number of methylsiloxane chains is too small, although the hydrophilicity of the softener emulsion can be improved after film formation, the softness deteriorates, and the excessive amino groups are oxidized and decomposed to form yellowing groups, which causes the fabric to yellow.
[0015] Furthermore, in step S1 of the method for preparing the super hydrophilic softener emulsion, the molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane is 14:8:23.
[0016] Furthermore, the catalyst in step S1 of the method for preparing the super hydrophilic softener emulsion is a sodium hydroxide aqueous solution, and the pH value of the sodium hydroxide aqueous solution is 8.5-9.0.
[0017] Furthermore, the emulsifier in step S2 of the preparation method of the super hydrophilic softener emulsion is composed of nonylphenol polyoxyethylene ether and castor oil polyoxyethylene ether in a mass ratio of 3-5:7-9, and the amount of the emulsifier is 20-25% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
[0018] Furthermore, the modifier in step S2 of the preparation method of the super hydrophilic softener emulsion is methyl allyl polyoxyethylene ether, and the amount of the modifier is 8-13% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane.
[0019] The amount of modifier used has an important influence on the hydrophilicity of the softener emulsion. When the amount of modifier used is too large or too small, the hydrophilicity of the softener emulsion will decrease.
[0020] Furthermore, in the step S2 of the method for preparing the super hydrophilic softener emulsion, the amount of the modifier used is 10% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
[0021] Furthermore, the organic acid in step S3 of the method for preparing the super hydrophilic softener emulsion is one of citric acid, tartaric acid and glacial acetic acid.
[0022] The invention also provides a super-hydrophilic softener emulsion prepared by using the preparation method of the super-hydrophilic softener emulsion.
[0023] Compared with the prior art, the super hydrophilic softener emulsion and the preparation method thereof provided by the present invention have the following technical advantages:
[0024] (1) The present invention uses γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane to polymerize to form the main chain of the polymer compound, introduces amino groups and hydroxyl groups into the molecular structure, and controls the dosage ratio of the three monomers to make the prepared super hydrophilic softener emulsion have excellent hydrophilic properties and softness after film formation;
[0025] (2) The present invention uses a polyether modifier to modify the amino silicone oil, which can further improve the hydrophilicity of the super hydrophilic softener emulsion;
[0026] (3) The preparation method of the super hydrophilic softener emulsion provided by the present invention is simple and easy, the raw materials are readily available, and it is easy to realize industrial production, and has broad application prospects. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. Those skilled in the art can make various modifications based on the basic idea of the present invention, but as long as they do not deviate from the basic idea of the present invention, they are all within the scope of the present invention.
[0028] In this specific embodiment, the model of the nonylphenol polyoxyethylene ether in the emulsifier is TX-12, and the model of the castor oil polyoxyethylene ether is EL-30.
[0029] Example 1. A method for preparing a super hydrophilic softener emulsion
[0030] The preparation method of the super hydrophilic softener emulsion comprises the following steps:
[0031] S1. γ-aminopropyltriethoxysilane and tetra(hydroxyethyl)silane were added to water respectively, stirred and hydrolyzed, and then added to the reactor, nitrogen was introduced, octamethylcyclotetrasiloxane was added, the temperature was raised to 80°C, an aqueous sodium hydroxide solution with a pH value of 8.5 was added, the temperature was continued to rise to 140°C, the reaction was kept warm for 2h, unreacted monomers were removed by vacuum, and the aminosilicone oil was obtained; the molar mass ratio of the γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane was 13:6:21;
[0032] S2. Add an emulsifier to the amino silicone oil obtained in step S1, stir evenly and heat to 80°C, add methyl allyl polyoxyethylene ether dropwise while stirring, keep warm for 5 hours after the addition is completed, and cool to 25°C to obtain modified amino silicone oil; the emulsifier is composed of nonylphenol polyoxyethylene ether and castor oil polyoxyethylene ether in a mass ratio of 3:7; the amount of the emulsifier is 20% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane; the amount of methyl allyl polyoxyethylene ether is 8% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane;
[0033] S3. Add citric acid to the modified amino silicone oil obtained in step S2 to adjust the pH value to 6.
[0034] Example 2. A method for preparing a super hydrophilic softener emulsion
[0035] The preparation method of the super hydrophilic softener emulsion comprises the following steps:
[0036] S1. γ-aminopropyltriethoxysilane and tetra(hydroxyethyl)silane were added to water respectively, stirred and hydrolyzed, and then added to the reactor, nitrogen was introduced, octamethylcyclotetrasiloxane was added, the temperature was raised to 85°C, an aqueous sodium hydroxide solution with a pH value of 9.0 was added, the temperature was continued to rise to 145°C, the reaction was kept warm for 3h, unreacted monomers were removed by vacuum, and the aminosilicone oil was obtained; the molar mass ratio of the γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane was 15:10:24;
[0037] S2. Add an emulsifier to the amino silicone oil obtained in step S1, stir evenly and heat to 90°C, add methyl allyl polyoxyethylene ether dropwise while stirring, keep warm for 4 hours after the addition is completed, and cool to 30°C to obtain modified amino silicone oil; the emulsifier is composed of nonylphenol polyoxyethylene ether and castor oil polyoxyethylene ether in a mass ratio of 5:9; the amount of the emulsifier is 5% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane; the amount of methyl allyl polyoxyethylene ether is 13% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane;
[0038] S3. Add tartaric acid to the modified amino silicone oil obtained in step S2 to adjust the pH value to 7.
[0039] Example 3. A method for preparing a super hydrophilic softener emulsion
[0040] The preparation method of the super hydrophilic softener emulsion comprises the following steps:
[0041] S1. γ-aminopropyltriethoxysilane and tetra(hydroxyethyl)silane were added to water respectively, stirred and hydrolyzed, and then added to the reactor, nitrogen was introduced, octamethylcyclotetrasiloxane was continued to be added, the temperature was raised to 82°C, an aqueous sodium hydroxide solution with a pH value of 8.8 was added, the temperature was continued to be raised to 143°C, the reaction was kept warm for 2.5 hours, unreacted monomers were removed by vacuum, and the aminosilicone oil was obtained; the molar mass ratio of the γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane was 14:8:23;
[0042] S2. Add an emulsifier to the amino silicone oil obtained in step S1, stir evenly and heat to 86°C, add methyl allyl polyoxyethylene ether dropwise while stirring, keep warm for 4.5 hours after the addition is completed, cool to 28°C, and obtain modified amino silicone oil; the emulsifier is composed of nonylphenol polyoxyethylene ether and castor oil polyoxyethylene ether in a mass ratio of 5:7; the amount of the emulsifier is 22% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane; the amount of methyl allyl polyoxyethylene ether is 10% of the total mass of γ-aminopropyl triethoxysilane, tetra(hydroxyethyl) silane and octamethylcyclotetrasiloxane;
[0043] S3. Add glacial acetic acid to the modified amino silicone oil obtained in step S2 to adjust the pH value to 6-7.
[0044] Comparative Example 1
[0045] The preparation method of the softener emulsion in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of γ-aminopropyltriethoxysilane is used instead of tetra(hydroxyethyl)silane in step S1 of this comparative example.
[0046] Comparative Example 2
[0047] The preparation method of the softener emulsion in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the molar mass ratio of γ-aminopropyltriethoxysilane, tetrakis(hydroxyethyl)silane and octamethylcyclotetrasiloxane in step S1 of this comparative example is 6:19:11.
[0048] Comparative Example 3
[0049] The preparation method of the softener emulsion in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the molar mass ratio of γ-aminopropyltriethoxysilane, tetrakis(hydroxyethyl)silane and octamethylcyclotetrasiloxane in step S1 of this comparative example is 4:11:2.
[0050] Comparative Example 4
[0051] The preparation method of the softener emulsion in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the amount of methyl allyl polyoxyethylene ether used in step S2 of this comparative example is 2% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
[0052] Comparative Example 5
[0053] The preparation method of the softener emulsion in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that the amount of methyl allyl polyoxyethylene ether used in step S2 of this comparative example is 22% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
[0054] Comparative Example 6
[0055] The preparation method of the softener emulsion in this comparative example is similar to that in Example 3. The difference between this comparative example and Example 3 is that an equal amount of polyoxyethylene methyl glycidyl ether is used instead of methyl allyl polyoxyethylene ether in step S2 of this comparative example.
[0056] Test Example 1: Performance Test
[0057] Test samples: softeners prepared in Examples 1-3 and Comparative Examples 1-6;
[0058] Test method: Prepare the test sample into 50g / L working solution, and finish the white pure cotton fabric through a dip-and-bind process. The setting temperature is 170℃, the setting time is 90s, and the fabric is tested after regaining moisture for 1h after finishing.
[0059] Hydrophilicity test: Use a standard dropper to drop one drop of water from a height of 10 cm from the fabric onto the horizontally spread fabric surface, and measure the time taken for the water to completely penetrate the fabric surface.
[0060] Softness test: Determine the bending stiffness of the fabric with reference to ASTM-D1388-08 (2022) "Standard Test Method for Fabric Stiffness".
[0061] Test results: The test results are shown in Table 1.
[0062] Table 1 Hydrophilicity and softness test results
[0063]
[0064] As shown in Table 1, the water absorption time of the super hydrophilic softener emulsion provided by the present invention after forming a film on the fabric surface is 2-5s, and the bending stiffness is 0.0125-0.0186g·cm 2 / cm, therefore, the super hydrophilic softener emulsion provided by the present invention has good hydrophilicity and softness after film formation. Among them, the super hydrophilic softener emulsion prepared in Example 3 has the shortest water absorption time after film formation and the smallest bending rigidity, which is the best embodiment of the present invention.
[0065] Compared with Example 3, in step S1 of comparative example 1, an equal amount of γ-aminopropyltriethoxysilane is used to replace tetra(hydroxyethyl)silane, but the hydrophilicity of the obtained softener emulsion after film formation is significantly worsened, which indicates that tetra(hydroxyethyl)silane can introduce hydroxyl groups into the molecular structure of amino silicone oil, thereby greatly improving the hydrophilicity of the softener emulsion; in comparative examples 2 and 3, the molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane in step S1 is changed, but the hydrophilicity and softness of the obtained softener emulsion after film formation are reduced to varying degrees, which indicates that the molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane in the present invention is reduced. The molar mass ratio of silane to octamethylcyclotetrasiloxane is the key to controlling the hydrophilicity and softness of the softener, and the molar mass ratio range provided by the present invention has reached the optimization; in Comparative Examples 4 and 5, the amount of methyl allyl polyoxyethylene ether in step S2 is changed, but the hydrophilicity of the obtained softener emulsion after film formation is greatly reduced, which shows that the amount of the modifier has an important influence on the hydrophilicity of the softener emulsion; Comparative Example 6 uses an equal amount of polyoxyethylene methyl glycidyl ether instead of methyl allyl polyoxyethylene ether, but the hydrophilicity of the obtained softener emulsion after film formation is slightly reduced, which shows that not all polyether modifiers can achieve the technical effect of the present invention.
[0066] The above embodiments are merely illustrative of the preparation method of the present invention, and are not intended to limit the present invention. Any person skilled in the art may not modify the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the technical concept provided by the present invention are still covered by the claims of the present invention.
Claims
1. A method for preparing a super hydrophilic softener emulsion, characterized in that: The following steps are involved: S1. γ-aminopropyltriethoxysilane and tetra(hydroxyethyl)silane were added to water respectively, stirred and hydrolyzed, and then added to the reaction kettle, nitrogen was introduced, octamethylcyclotetrasiloxane was added, the temperature was raised to 80-85°C, a catalyst was added, the temperature was continued to be raised to 140-145°C, the temperature was kept for 2-3h, unreacted monomers were removed by vacuum, and the amino silicone oil was obtained; S2. Add an emulsifier to the amino silicone oil obtained in step S1, stir evenly and heat to 80-90°C, add a modifier dropwise while stirring, keep the reaction warm for 4-5h after the addition is complete, and cool to 25-30°C to obtain a modified amino silicone oil; S3. Add an organic acid to the modified amino silicone oil obtained in step S2 to adjust the pH value to 6-7 to obtain; The molar mass ratio of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane in step S1 is 13-15:6-10:21-24; the modifier in step S2 is methyl allyl polyoxyethylene ether, and the amount of the modifier is 8-13% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
2. The preparation method of super hydrophilic softener emulsion according to claim 1, characterized in that, The molar mass ratio of γ-aminopropyltriethoxysilane, tetrakis(hydroxyethyl)silane and octamethylcyclotetrasiloxane in step S1 is 14:8:
23.
3. The preparation method of super hydrophilic softener emulsion according to claim 1, characterized in that, The catalyst in step S1 is a sodium hydroxide aqueous solution, and the pH value of the sodium hydroxide aqueous solution is 8.5-9.
0.
4. The preparation method of super hydrophilic softener emulsion according to claim 1, characterized in that, The emulsifier in step S2 is composed of nonylphenol polyoxyethylene ether and castor oil polyoxyethylene ether in a mass ratio of 3-5:7-9, and the amount of the emulsifier is 20-25% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
5. The preparation method of super hydrophilic softener emulsion according to claim 1, characterized in that, The amount of the modifier used in step S2 is 10% of the total mass of γ-aminopropyltriethoxysilane, tetra(hydroxyethyl)silane and octamethylcyclotetrasiloxane.
6. The preparation method of super hydrophilic softener emulsion according to claim 1, characterized in that, The organic acid in step S3 is one of citric acid, tartaric acid and glacial acetic acid.
7. A super-hydrophilic softener emulsion prepared according to the preparation method of the super-hydrophilic softener emulsion according to any one of claims 1 to 6.
Citation Information
Patent Citations
Hydrophilic fabric softener
CN106498751A
Non-silicon hydrophilic softening agent, preparation method thereof and application of softening agent
CN110656500A
Preparation method of hyperbranched ternary polymerization organic silicon
CN104650363A
Water-retaining agent for improving concrete state and preparation method thereof
CN110606694A