A cross-linked polyetherimide dielectric film and its preparation method and application
By constructing a cross-linked network in a polyetherimide dielectric film, the problem of insufficient performance of polymer dielectrics under high temperatures and high fields is solved, stable operation and high energy storage density in extreme environments are achieved, and the process is simple and Environmentally friendly.
Patent Information
- Application Number
- CN202410393203.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-02
AI Technical Summary
Existing polymer dielectrics increase leakage current and conduction losses under high temperature and high field conditions, which cannot meet the application needs in extreme environments. It is also difficult to easily and effectively construct a cross-linked structure in organic polymers to improve capacitive performance.
A method for preparing a cross-linked polyetherimide dielectric film is used to perform a polymerization reaction by mixing dianhydrides, diamines and carboxyl-containing diamine monomers with anhydrous organic solvents, followed by an imidization reaction with a catalyst. Finally, decarboxylation and cross-linking are performed to form a dielectric film with a cross-linked network.
It achieves outstanding breakdown electric field strength and energy storage performance at 200°C and 250°C, reduces leakage current density, improves the high-temperature insulation performance and energy storage density of the dielectric film, and has a simple process, environmental friendliness, and compatibility Industrial production process.
Smart Images

Figure CN118290785B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of dielectric material preparation, and in particular to a cross-linked polyetherimide dielectric film and a preparation method and application thereof. Background Art
[0002] As an important component of electrical energy storage, dielectric capacitors play a vital role in high-power electronic power systems. In particular, with the rapid development of human society, capacitors with high temperature and high voltage resistance are indispensable to new energy vehicles, oil and gas exploration, and aerospace fields. For example, in new energy vehicles, the power inverter that works close to the engine requires the capacitor film of its basic components to operate stably above 140°C. Among them, organic film capacitors have become the preferred material in the field of electrostatic capacitors due to their advantages such as light weight, easy processing, low cost, high voltage resistance, easy integration and assembly processing, and no liquid medium.
[0003] However, commercial polymer capacitors on the market are difficult to operate stably in high temperature environments. For example, the operating temperature of biaxially oriented polypropylene (BOPP), a typical commercial polymer dielectric, does not exceed 105°C. Especially when the actual application temperature exceeds 85°C, the capacitance energy storage performance of BOPP deteriorates seriously. In order to improve the high-temperature capacitance energy storage performance of polymer dielectrics, researchers at home and abroad have developed polyimide dielectric materials with high glass transition temperatures (Tg). However, this type of material has a low thermal conductivity at 150°C and 300MVm. -1 Under the above high temperature and high field conditions, the leakage current increases and the conduction loss increases, which cannot meet the application requirements in extreme environments.
[0004] Patent CN111004507A discloses a method for preparing a cross-linked polyetherimide-based dielectric composite film, which uses a nano-ceramic powder with a core-shell structure as a filler, and introduces a cross-linkable organic functional group to the surface of the filler, so that it undergoes a cross-linking reaction with the polyetherimide matrix, thereby solving the compatibility problem between the inorganic phase and the organic phase. The prepared cross-linked polyetherimide-based dielectric composite film has a higher dielectric constant (εr) and lower dielectric loss (tanδ) over a wide temperature range. Although the dielectric composite film has excellent dielectric properties, its high-temperature capacitance performance needs to be optimized, which limits its application. Therefore, how to simply and effectively construct a cross-linked structure in an organic polymer and enable it to have excellent capacitance performance under extreme environments is the main technical challenge currently faced. Summary of the invention
[0005] The object of the present invention is to provide a cross-linked polyetherimide dielectric film and a preparation method and application thereof, so as to solve the problems existing in the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a cross-linked polyetherimide dielectric film, comprising the following preparation steps:
[0008] S1: mixing dianhydride, diamine, carboxyl-containing diamine monomer and anhydrous organic solvent to carry out polymerization reaction to obtain a carboxyl-functionalized polyetherimide acid precursor solution;
[0009] S2: mixing the precursor solution of step S1 with the catalyst, and performing an imidization reaction to obtain a polymer solution;
[0010] S3: The polymer solution of step S2 is allowed to stand, and then coated on a substrate, and further imidization is completed, and then decarboxylation cross-linking is performed to obtain a cross-linked polyetherimide dielectric film.
[0011] Optionally, the diamine comprises one or more of bis(4-aminophenyl)sulfone, 3,3'-diaminodiphenylsulfone, 1,3-phenylenediamine, 4,4'-diaminodiphenyl ether, and 1,4-phenylenediamine;
[0012] The dianhydride comprises one or more of bisphenol A type diether dianhydride, 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride;
[0013] The carboxyl-containing diamine monomer includes one or more of 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, and 3,5-diamino-4-methylbenzoic acid;
[0014] The anhydrous organic solvent comprises N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, m-phenol or dimethyl sulfoxide.
[0015] Optionally, the molar ratio of the dianhydride, diamine and carboxyl-containing diamine monomer is
[0016] (1~1.02)∶(0~0.4)∶(0.6~1.02).
[0017] Optionally, the molar ratio of the dianhydride to the anhydrous organic solvent is 1:20-30; and the molar ratio of the total moles of the diamine and the carboxyl-containing diamine monomer to the anhydrous organic solvent is 1:20-30.
[0018] Optionally, the polymerization reaction temperature is 10 to 30° C., and the polymerization reaction time is 20 to 30 hours.
[0019] Optionally, the solid content of the carboxyl functionalized polyetherimide acid precursor solution is 9-15%.
[0020] Optionally, the catalyst is isoquinoline, or a mixture of pyridine and acetic anhydride, the volume ratio of pyridine to acetic anhydride is 1:1; the temperature of the imidization reaction in step S2 is 140-200°C, and the time is 0.5-5h; the volume ratio of the catalyst to the precursor solution is 1:100-120.
[0021] Optionally, the standing time is 1 to 4 hours; the gradient temperature rise program of the imidization in step S3 is: 60 to 80°C / 2 to 3 hours, 90 to 110°C / 1 to 2 hours, 140 to 160°C / 0.8 to 1 hour, 180 to 220°C / 0.8 to 1 hour, 240 to 280°C / 0.8 to 1 hour; the temperature of the decarboxylation cross-linking is 330 to 380°C, and the time is 0.5 to 3 hours.
[0022] The present invention also provides a cross-linked polyetherimide dielectric film prepared by the above-mentioned preparation method, characterized in that the cross-linked polyetherimide dielectric film has a thickness of 8 to 20 μm.
[0023] The present invention also provides application of the cross-linked polyetherimide dielectric film in dielectric capacitors.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention adopts a "one-pot method" to prepare a cross-linked polyetherimide dielectric film with simple feeding, environmental friendliness, controllable cross-linking degree and excellent high-temperature energy storage performance. The preparation process is simple, and the reaction is carried out in the liquid phase. It is fully compatible with the current industrial production process of polyetherimide dielectric films. And the prepared cross-linked polyetherimide dielectric film has excellent thermal stability and mechanical properties, and has outstanding breakdown electric field strength and energy storage performance at 200°C and 250°C. The polyetherimide dielectric film manufactured by this preparation method can be expected to achieve under extreme environments (T=250°C, E>200MVm -1 )Stable operation.
[0026] 2. The fully organic cross-linked polyetherimide dielectric film obtained by the present invention constructs a cross-linked network through covalent bonds between chains or at the ends of the chains, thereby improving the thermal stability and Young's modulus performance of the polyetherimide dielectric film.
[0027] 3. The present invention introduces many discretely distributed deep traps inside the polymer dielectric by introducing carboxyl groups and cross-linked networks. Under high temperature and high field, the free electrons excited by heat or injected by electrodes are captured or bound by these deep traps, which reduces the leakage current density of the material, thereby improving the high temperature insulation performance of the dielectric film.
[0028] 4. The cross-linked polyetherimide dielectric film prepared by the present invention can achieve an energy storage density of 4.7 to 5.2 J / cm at 200°C and 90% energy storage efficiency. 3 , at 250℃, 90% efficiency can reach 2.8~3.46J / cm 3 , significantly exceeding existing dielectric materials; and the glass transition temperature (T g ), Young's modulus, leakage current and energy storage performance are all improved, and the comprehensive dielectric properties are good. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The chemical reaction flow chart of Example 1;
[0030] Figure 2 The figure is a graph showing the effect of the cross-linked network in the cross-linked polyetherimide dielectric films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 on the thermal stability of polyetherimide;
[0031] Figure 3 The effect of the cross-linked network in the cross-linked polyetherimide dielectric films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 on the mechanical properties of polyetherimide;
[0032] Figure 4 The left side shows the leakage current density of the cross-linked polyetherimide dielectric films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 at 200° C., and the right side shows the leakage current density of the cross-linked polyetherimide dielectric films prepared in Comparative Example 1 and Example 2 at 250° C.;
[0033] Figure 5 The left side shows the capacitance energy storage performance of the cross-linked polyetherimide dielectric films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 at 200°C, and the right side shows the capacitance energy storage performance of the cross-linked polyetherimide dielectric films prepared in Comparative Example 1 and Example 2 at 250°C. DETAILED DESCRIPTION
[0034] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0035] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0036] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0039] The present invention provides a method for preparing a cross-linked polyetherimide dielectric film, comprising the following preparation steps:
[0040] S1: mixing dianhydride, diamine, carboxyl-containing diamine monomer and anhydrous organic solvent to carry out polymerization reaction to obtain a carboxyl-functionalized polyetherimide acid precursor solution;
[0041] S2: mixing the precursor solution of step S1 with the catalyst, and performing an imidization reaction to obtain a polymer solution;
[0042] S3: The polymer solution of step S2 is allowed to stand, and then coated on a substrate, and further imidization is completed, and then decarboxylation cross-linking is performed to obtain a cross-linked polyetherimide dielectric film.
[0043] In the present invention, the diamine comprises one or more of bis(4-aminophenyl)sulfone, 3,3'-diaminodiphenylsulfone, 1,3-phenylenediamine, 4,4'-diaminodiphenyl ether, and 1,4-phenylenediamine, preferably one or more of 1,3-phenylenediamine, 4,4'-diaminodiphenyl ether, and 1,4-phenylenediamine, more preferably one or more of 4,4'-diaminodiphenyl ether and 1,4-phenylenediamine, most preferably bis(4-aminophenyl)sulfone;
[0044] The dianhydride comprises one or more of bisphenol A type diether dianhydride, 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, and 3,3,4,4-diphenylsulfonetetracarboxylic anhydride, preferably one or more of 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, and 3,3,4,4-diphenylsulfonetetracarboxylic anhydride, more preferably one or more of 3,3',4,4'-benzophenonetetracarboxylic anhydride and 3,3,4,4-diphenylsulfonetetracarboxylic anhydride, and most preferably bisphenol A type diether dianhydride;
[0045] The carboxyl group-containing diamine monomer comprises one or more of 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, and 3,5-diamino-4-methylbenzoic acid, preferably one or more of 3,4-diaminobenzoic acid and 3,5-diamino-4-methylbenzoic acid, and most preferably 3,5-diaminobenzoic acid;
[0046] The anhydrous organic solvent comprises N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, meta-phenol or dimethyl sulfoxide, preferably N,N-dimethylacetamide, N,N-dimethylformamide, meta-phenol or dimethyl sulfoxide, further preferably N,N-dimethylformamide, meta-phenol or dimethyl sulfoxide, and most preferably N,N-dimethylformamide.
[0047] In the present invention, the anhydrous organic solvent requires a molecular sieve to remove water molecules in the solvent.
[0048] In the present invention, the molar ratio of the dianhydride, diamine and carboxyl-containing diamine monomer is
[0049] (1~1.02):(0~0.4):(0.6~1.02), preferably 1.01:0.2:0.8.
[0050] In the present invention, the content of the carboxyl group-containing diamine accounts for 60 to 100% of the total diamine content, preferably 70 to 90%, and more preferably 80%.
[0051] In the present invention, the molar ratio of the dianhydride to the anhydrous organic solvent is 1:20-30, preferably 1:22-28, and more preferably 1:25-26; the molar ratio of the total molar number of the diamine and the carboxyl-containing diamine monomer to the anhydrous organic solvent is 1:20-30, preferably 1:22-28, and more preferably 1:25-26.
[0052] In the present invention, the polymerization reaction temperature is 10-30°C, preferably 12-28°C, more preferably 15-25°C, and more preferably 20-23°C. The polymerization reaction time is 20-30h, preferably 22-28h, and more preferably 25-26h.
[0053] In the present invention, the solid content of the carboxyl functionalized polyetherimide acid precursor solution is 9 to 15%, preferably 10 to 14%, and more preferably 12 to 13%.
[0054] In the present invention, the mixing method of step S1 is: firstly, dianhydride and anhydrous organic solvent are mixed to obtain an anhydride solution, and then diamine and carboxyl diamine monomer are mixed with anhydrous organic solvent to obtain a diamine mixed solution, and the diamine mixed solution is added to the anhydride solution four times every 10 to 15 minutes to ensure that it is completely dissolved, and after the diamine mixed solution is added, a polymerization reaction is carried out to obtain a carboxyl functionalized polyetherimide acid precursor polymer solution.
[0055] In the present invention, the catalyst is isoquinoline, or a mixture of pyridine and acetic anhydride, wherein the volume ratio of pyridine to acetic anhydride is 1:1;
[0056] The temperature of the imidization reaction in step S2 is 140-200° C., preferably 150-180° C., more preferably 160-170° C., and the time is 0.5-5 h, preferably 1-4 h, more preferably 2-3 h;
[0057] The volume ratio of the catalyst to the precursor solution is 1:100-120, preferably 1:105-115, and more preferably 1:108-110.
[0058] In the present invention, the standing time is 1 to 4 hours, preferably 2 to 3 hours; the purpose of standing is to remove the gas in the viscous solution.
[0059] In the present invention, the gradient temperature rise program of the imidization in step S3 is: 60-80°C / 2-3h, 90-110°C / 1-2h, 140-160°C / 0.8-1h, 180-220°C / 0.8-1h, 240-280°C / 0.8-1h; the temperature of the decarboxylation cross-linking is 330-380°C, preferably 340-370°C, further preferably 350-360°C, and the time is 0.5-3h, preferably 1-2h.
[0060] In the present invention, the purpose of the gradient temperature increase is to remove a large amount of solvent and catalyst and to complete the final imidization.
[0061] In the present invention, the chemical imidization and the gradient temperature imidization work together to make the imidization of the precursor solution more complete.
[0062] In the present invention, the substrate is one of a glass plate, a steel material, and a polyimide film.
[0063] In the present invention, after the decarboxylation crosslinking in step S2 is completed, the film is peeled off with warm water and then dried to obtain a cross-linked polyetherimide film; the drying temperature is 100-150°C, preferably 110-140°C, and more preferably 120-130°C.
[0064] The present invention also provides a cross-linked polyetherimide dielectric film prepared by the above-mentioned preparation method, characterized in that the thickness of the cross-linked polyetherimide dielectric film is 8 to 20 μm, preferably 10 to 18 μm, more preferably 12 to 16 μm, and further preferably 14 to 15 μm.
[0065] The present invention also provides application of the cross-linked polyetherimide dielectric film in dielectric capacitors.
[0066] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0067] Example 1
[0068] Preparation of carboxyl-containing polyetheramic acid (PAA) prepolymer solution: weigh 0.384 mmol of bisphenol A diether dianhydride, stir and dissolve it in 10 mmol of anhydrous N, N-dimethylacetamide; then weigh 0.1536 mmol (4-aminophenyl) sulfone and 0.2304 mmol 3,5-diaminobenzoic acid, prepare and dissolve them in 10 mmol of anhydrous N, N-dimethylacetamide to obtain a diamine mixed solution. Every 10 to 15 minutes, the diamine mixed solution is added to the anhydride solution in four times to ensure that it is completely dissolved. After the diamine mixed solution is added, stir and react at 20°C for 22 hours to obtain a viscous PAA solution with a solid content of 13%.
[0069] Preparation of cross-linked polyetherimide dielectric film: add 0.02 ml of isoquinoline to the viscous PAA solution and react at 160°C for 2 hours to obtain a polyetherimide solution, cool it down, and let it stand for 2 hours to remove excess gas, then coat it on a clean steel plate, and increase the temperature in ascending order of 70°C for 3 hours, 150°C for 1 hour, 250°C for 1 hour, and 280°C for 2 hours to remove a large amount of N,N-dimethylacetamide and isoquinoline, then place the film at 360°C for 1 hour for moderate thermal cross-linking, finally peel off the film with warm water, and then place it at 120°C for drying to obtain a cross-linked polyetherimide dielectric film. The thickness of the cross-linked polyetherimide dielectric film is 10μm, recorded as 60PEI-PS.
[0070] Figure 1 This is the chemical reaction flow chart of Example 1 of the present invention, in which a polyetherimide monomer with a carboxyl group is reacted to synthesize a polyetherimide acid prepolymer with a carboxyl group at the end or side chain, and then a high-temperature energy storage polyetherimide dielectric film is prepared by chemical imidization, coating and heat treatment.
[0071] Example 2
[0072] The only difference from Example 1 is that 0.077 mmol (4-aminophenyl) sulfone (DPS) and 0.307 mmol 3,5-diaminobenzoic acid (DBA) are weighed and recorded as 80 PEI-PS.
[0073] Example 3
[0074] The only difference from Example 1 is that 0 mmol (4-aminophenyl) sulfone (DPS) and 0.384 mmol 3,5-diaminobenzoic acid (DBA) were weighed and recorded as 100 PEI-PS.
[0075] Comparative Example 1
[0076] The only difference from Example 1 is that 0.384 mmol (4-aminophenyl) sulfone (DPS) and 0 mmol 3,5-diaminobenzoic acid (DBA) are weighed and recorded as PEI-PS.
[0077] Comparative Example 2
[0078] The only difference from Example 1 is that 0.307 mmol (4-aminophenyl) sulfone (DPS) and 0.077 mmol 3,5-diaminobenzoic acid (DBA) were weighed and recorded as 20PEI-PS.
[0079] Comparative Example 3
[0080] The only difference from Example 1 is that 0.2304 mmol (4-aminophenyl) sulfone (DPS) and 0.1536 mmol 3,5-diaminobenzoic acid (DBA) were weighed and recorded as 40PEI-PS.
[0081] The electrical properties of the dielectric materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested by sandwiching the prepared dielectric films between two metal masks with circular holes of 2 mm in diameter, and symmetrically sputtering gold electrodes on the upper and lower surfaces. The performance tests were conducted using a ferroelectric workstation and a differential scanning calorimeter.
[0082] Figure 2 1 is a graph showing the effect of the cross-linked network on the thermal stability of the cross-linked polyetherimide dielectric film prepared in Examples 1 to 3 and Comparative Examples 1 to 3. Figure 2It can be seen that crosslinking between molecular chains is beneficial to improving the heat resistance of polyetherimide films, and as the content of diamine with carboxyl groups increases, the crosslinking degree induced by carboxyl groups increases, and the glass transition temperature (Tg) increases;
[0083] Figure 3 The effect of the cross-linked network in the cross-linked polyetherimide dielectric film prepared in Examples 1 to 3 and Comparative Examples 1 to 3 on the mechanical properties of polyetherimide is shown in FIG. Figure 3 The results of Young's modulus and nanoindentation show that cross-linking has greatly improved the mechanical properties of the film, increasing the Young's modulus from 4.00 GPa of PEI-PS to 4.75 GPa of 100 PEI-PS. The increase in Young's modulus is very helpful in avoiding electromechanical breakdown of the film.
[0084] The fully organic cross-linked polyetherimide dielectric film obtained by the invention constructs a cross-linked network through covalent bonds between chains or at chain ends, thereby improving the thermal stability and Young's modulus performance of the polyetherimide.
[0085] Figure 4 The left side shows the leakage current density of the cross-linked polyetherimide dielectric film prepared in Examples 1 to 3 and Comparative Examples 1 to 3 at 200°C, and the right side shows the leakage current density of the cross-linked polyetherimide dielectric film prepared in Comparative Example 1 and Example 2 at 250°C; Figure 4 It can be seen from the left that at 200°C, the non-cross-linked PEI-PS has the highest leakage current density and the largest fitted jumping distance. In comparison, the leakage current density of the carboxyl-containing and cross-linked PEI-PS is well suppressed, and the jumping distance is reduced, which indicates that the cross-linked network and the non-cross-linked carboxyl groups can act as carrier traps to capture and suppress the transport of carriers. Figure 4 It can be seen from the right that at 250°C, the fitted jumping distance of 80PEI-PS is much smaller than the fitted jumping distance of PEI-PS, which shows that even under the harsh environment of 250°C, PEI-PS modified by this cross-linking method has excellent insulation properties.
[0086] Figure 5 The left side shows the capacitance energy storage performance of the cross-linked polyetherimide dielectric films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 at 200°C, and the right side shows the capacitance energy storage performance of the cross-linked polyetherimide dielectric films prepared in Comparative Example 1 and Example 2 at 250°C; Figure 5 It can be seen that the cross-linked polyetherimide dielectric film prepared by the present invention can achieve an energy storage density of 4.7 to 5.2 J / cm at 200°C and 90% energy storage efficiency. 3 , at 250℃, 90% efficiency can reach 2.8~3.46J / cm 3 , significantly exceeding existing dielectric materials.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a cross-linked polyetherimide dielectric film, characterized in that: The preparation steps include: S1: mixing dianhydride, diamine, carboxyl-containing diamine monomer and anhydrous organic solvent to carry out polymerization reaction to obtain a carboxyl-functionalized polyetherimide acid precursor solution; The molar ratio of the dianhydride, the diamine and the carboxyl group-containing diamine monomer is (1-1.02): (0-0.4): (0.6-1.02); S2: mixing the precursor solution of step S1 with the catalyst, and performing an imidization reaction to obtain a polymer solution; S3: allowing the polymer solution of step S2 to stand, and then coating it on a substrate, further completing imidization, and then performing decarboxylation crosslinking to obtain a crosslinked polyetherimide dielectric film; The temperature of the decarboxylation cross-linking is 330-380° C., and the time is 0.5-3 h.
2. The method for preparing a cross-linked polyetherimide dielectric film according to claim 1, characterized in that: The diamine comprises one or more of bis(4-aminophenyl)sulfone, 3,3'-diaminodiphenylsulfone, 1,3-phenylenediamine, 4,4'-diaminodiphenyl ether, and 1,4-phenylenediamine; The dianhydride comprises one or more of bisphenol A type diether dianhydride, 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride; The carboxyl-containing diamine monomer includes one or more of 3,5-diaminobenzoic acid, 3,4-diaminobenzoic acid, and 3,5-diamino-4-methylbenzoic acid; The anhydrous organic solvent comprises N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, m-phenol or dimethyl sulfoxide.
3. The method for preparing a cross-linked polyetherimide dielectric film according to claim 2, characterized in that: The molar ratio of the dianhydride to the anhydrous organic solvent is 1:20-30; the molar ratio of the total molar number of the diamine and the carboxyl-containing diamine monomer to the anhydrous organic solvent is 1:20-30.
4. The method for preparing a cross-linked polyetherimide dielectric film according to claim 1, characterized in that: The polymerization reaction temperature is 10-30° C., and the polymerization reaction time is 20-30 hours.
5. The method for preparing a cross-linked polyetherimide dielectric film according to claim 1, characterized in that: The solid content of the carboxyl functionalized polyetherimide acid precursor solution is 9-15%.
6. The method for preparing a cross-linked polyetherimide dielectric film according to claim 1, characterized in that: The catalyst is isoquinoline, or a mixture of pyridine and acetic anhydride, the volume ratio of pyridine to acetic anhydride is 1:1; the temperature of the imidization reaction in step S2 is 140-200°C, and the time is 0.5-5h; the volume ratio of the catalyst to the precursor solution is 1:100-120.
7. The method for preparing a cross-linked polyetherimide dielectric film according to claim 1, characterized in that: The standing time is 1~4h; the gradient temperature rising program of the imidization in step S3 is: 60~80℃ / 2~3h, 90~110℃ / 1~2h, 140~160℃ / 0.8~1h, 180~220℃ / 0.8~1h, 240~280℃ / 0.8~1h.
8. A cross-linked polyetherimide dielectric film prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The cross-linked polyetherimide dielectric film has a thickness of 8-20 μm.
9. Use of the cross-linked polyetherimide dielectric film according to claim 8 in a dielectric capacitor.