A kind of aging-resistant PET film and preparation method thereof

By forming a double-layer coating structure on the PET film and using materials such as modified polyvinylidene fluoride and photosensitive oligomers, the problem of poor aging resistance of the PET film in lithium batteries is solved, and the aging resistance of the film is significantly improved. performance and interface affinity, extending service life and improving battery stability and performance.

CN118290798BActive Publication Date: 2024-10-25扬州博恒新能源材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410449621.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-10-25
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

The existing PET film has poor aging resistance during high-temperature cycling of lithium batteries, is easily degraded, and has poor interface affinity with the copper layer or aluminum layer, affecting battery performance and cycle life.

Method used

Adopting a double-layer coating structure, PVDF slurry and PVDF-HFP slurry are respectively coated on the PET base film, combined with materials such as modified polyvinylidene fluoride, photosensitive oligomers, alumina and modified clay, to enhance The mechanical properties, high temperature resistance and interface affinity of the film form an aging-resistant PET film.

Benefits of technology

Significantly improve the coating adhesion, electrolyte resistance and thermal stability of the aging-resistant PET film, enhance the interface affinity with the copper layer or aluminum layer, extend the service life and improve the stability and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of film technology, specifically to an anti-aging PET film and a preparation method thereof. The method comprises the following steps: step 1: adding polyvinylidene fluoride, modified polyvinylidene fluoride, photosensitive oligomer, aluminum oxide, modified clay, and initiator to dihydro-levo-glucose ketone in sequence, homogenizing, and obtaining PVDF slurry; step 2: adding poly(vinylidene fluoride-co-hexafluoropropylene), modified polyvinylidene fluoride, dimethylaminoethyl methacrylate, modified clay, water-based additive, and initiator to deionized water in sequence to obtain PVDF-HFP slurry; step 3: first coating the surface of the PET base film with PVDF slurry, and irradiating with ultraviolet light for 10 to 15 seconds; coating PVDF-HFP slurry, and irradiating with ultraviolet light for 20 to 30 seconds; then placing in deionized water, extracting and cleaning; drying at 60 to 80 ° C to obtain an anti-aging PET film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thin films, in particular to an anti-aging PET film and a preparation method thereof. Background Art

[0002] In recent years, the rapid development of electric vehicles and energy storage systems has promoted the research of various advanced battery materials. Among them, the current collector is an indispensable and important component in lithium-ion batteries. In current research, compared with the traditional lithium-ion battery in which the negative current collector and the positive current collector are prepared separately and then assembled, the new composite current collector has higher safety, higher energy density, higher assembly efficiency and lower cost, and has become the only way for the iteration of lithium-ion batteries.

[0003] The composite current collector is a composite material that uses a polymer film as an intermediate layer to integrate the negative electrode and the positive electrode. Since the polymer film undertakes the negative electrode and the positive electrode, this also means that the performance of the polymer film plays an important role in the battery cycle performance. At present, polymer films generally include polyethylene terephthalate film (PET film), polypropylene film (PP film), and polyimide film (PI film). Among them, the PI film has a high cost and is still not mass-produced as a current collector film. The PP film has low toughness and poor adhesion to the copper layer. In comparison, the melting point of the PET film can reach 260°C. It has the characteristics of a polar material and can have an interface with the copper layer or the aluminum layer. It has better mechanical properties and is easy to be used as an intermediate layer material. However, its aging resistance is poor. During the high-temperature cycle of the lithium battery, it degrades in the electrolyte and cannot meet the requirements of the battery cycle life. There are defects in applications such as automobiles. The coating of inorganic fillers can be used to improve its aging resistance, but there are problems such as decreased interfacial adhesion during the cycle and poor interfacial affinity with the copper layer or the aluminum layer, which affects the battery performance.

[0004] In summary, solving the above problems and preparing an aging-resistant PET film has important application value in composite current collectors. Summary of the invention

[0005] The object of the present invention is to provide an aging-resistant PET film and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing an aging-resistant PET film comprises the following steps:

[0008] Step 1: adding polyvinylidene fluoride, modified polyvinylidene fluoride, photosensitive oligomer, alumina, modified clay, and initiator to dihydro-levorotatory glucosone in sequence, and homogenizing to obtain PVDF slurry;

[0009] Step 2: Add poly(vinylidene fluoride-co-hexafluoropropylene), modified polyvinylidene fluoride, dimethylaminoethyl methacrylate, modified clay, water-based additive, and initiator to deionized water in sequence, and homogenize to obtain PVDF-HFP slurry;

[0010] Step 3: first coat the surface of the PET base film with PVDF slurry and expose it to ultraviolet light for 10 to 15 seconds; then coat it with PVDF-HFP slurry and expose it to ultraviolet light for 20 to 30 seconds; then place it in deionized water for extraction and cleaning; and dry it at 60 to 80°C to obtain an aging-resistant PET film.

[0011] More optimally, the PVDF slurry comprises the following components: by weight, 2 to 3 parts of polyvinylidene fluoride, 3 to 4 parts of modified polyvinylidene fluoride, 5 to 8 parts of photosensitive oligomer, 32 to 40 parts of alumina, 8 to 10 parts of modified clay, 0.1 to 0.2 parts of initiator, and 100 to 120 parts of dihydro-levulinic ketone.

[0012] More optimally, the PVDF-HFP slurry includes the following components: by weight, 20 to 22 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 5 to 8 parts of modified polyvinylidene fluoride, 4 to 6 parts of dimethylaminoethyl methacrylate, 2 to 4 parts of modified clay, 8 to 10 parts of water-based additives, 0.1 to 0.2 parts of initiator, and 100 to 120 parts of deionized water.

[0013] More optimally, the preparation method of the modified polyvinylidene fluoride comprises the following steps:

[0014] S1: Add β-cyclodextrin to DMF, add N,N'-carbonyldiimidazole, and stir at 20-25°C for 2-3 hours; add 1-amino-2-vinylcyclopropanecarboxylic acid, and continue stirring and reacting for 20-24 hours to obtain modified cyclodextrin;

[0015] S2: adding polyvinylidene fluoride to DMF, stirring at 20-25°C for 2-3 hours, and washing with water; transferring it to a mixed aqueous solution A containing potassium permanganate and potassium hydroxide, stirring at 20-25°C for 8-10 hours, and washing with water; transferring it to a mixed aqueous solution B containing sulfuric acid and sodium bisulfite, stirring at 20-25°C for 2-3 hours, washing with water, and drying to obtain hydroxylated polyvinylidene fluoride;

[0016] S3: Add acrylic acid to ethylene glycol, add hydroxylated polyvinylidene fluoride, modified cyclodextrin, and concentrated sulfuric acid; raise the temperature to 90-95°C, stir and react for 4-6 hours, wash with water, and dry to obtain modified polyvinylidene fluoride.

[0017] More optimally, in the raw materials of the modified cyclodextrin, the mass ratio of β-cyclodextrin, N,N'-carbonyldiimidazole, and 1-amino-2-vinylcyclopropanecarboxylic acid is 1:(0.4~0.43):(0.3~0.35); the raw materials of the modified polyvinylidene fluoride include the following components: by weight, 20 parts of hydroxylated polyvinylidene fluoride, 16~17 parts of acrylic acid, 7~8 parts of ethylene glycol, 5~6 parts of modified cyclodextrin, and 4~5 parts of concentrated sulfuric acid.

[0018] More optimally, in the mixed aqueous solution A, the content of potassium permanganate is 4-4.2wt%, and the content of potassium hydroxide is 19.8-20wt%; in the mixed aqueous solution B, the content of sulfuric acid is 4.5-5wt%, and the content of sodium bisulfite is 4.5-5wt%.

[0019] More optimally, the preparation method of the photosensitive oligomer is: mix poly (neopentyl adipate) glycol ester and 2,2,3,3-tetrafluoro-1,4-butanediol, evacuate at 95-100°C and stir for 40-60 minutes; cool to 70-75°C, add diisocyanate and organotin, raise the temperature to 85-90°C for reaction, add 1,3,5-cyclohexanetriol when the -NCO content is 8-9%, continue to react until the -NCO content is 2.5-3.5%, add pentaerythritol triacrylate, and react for another 2-2.5 hours to obtain a photosensitive oligomer.

[0020] More optimally, the raw materials of the photosensitive oligomer include the following components: by weight, 16 to 18 parts of polyneopentyl adipate, 2 to 4 parts of 2,2,3,3-tetrafluoro-1,4-butanediol, 8 to 10 parts of diisocyanate, 0.01 to 0.02 parts of organotin, 12 to 14 parts of 1,3,5-cyclohexanetriol, and 7 to 8 parts of pentaerythritol triacrylate.

[0021] More optimally, the preparation method of the modified clay is: ultrasonically dispersing the clay in an ethanol aqueous solution, adding hexadecyltrimethylammonium bromide and ultrasonically dispersing it again, then heating it to 80-85°C, stirring for 4-5 hours, filtering, washing with water, and freeze-drying to obtain a powder; adding the powder and tetrabutyl titanate to xylene in sequence, stirring at room temperature for 2-3 hours, adding a xylene solution containing urushiol, heating to 80-85°C for reaction for 1-1.5 hours, then heating to 115-120°C and stirring for 1-2 hours, continuing to heat to 125-135°C and stirring for 0.5-1 hour, cooling, washing with water, and drying to obtain the modified clay;

[0022] Among them, the mass ratio of clay to hexadecyltrimethylammonium bromide is 10:(2.5~3.5); the mass ratio of powder, tetrabutyl titanate and urushiol is 10:(4~4.2):(7~7.5).

[0023] More optimally, in an aging-resistant PET film prepared by a method for preparing an aging-resistant PET film, the thickness of the PET base film is 3-6 μm; the coating thickness of the PVDF slurry is 2-3 μm, and the coating thickness of the PVDF-HFP slurry is 0.5-1 μm.

[0024] Compared with the prior art, the present application has the following beneficial effects: in the scheme, compared with the common single-layer coating, the scheme forms a double-layer coating by introducing two slurries and coating them on the PET base film in sequence, thereby obtaining an aging-resistant PET film, which has excellent coating adhesion. At the same time, the film has excellent aging resistance in the electrolyte, and ensures the interfacial affinity between the film and the copper layer or aluminum layer, thereby increasing its applicability in the composite current collector.

[0025] In the scheme, PVDF slurry is obtained by mixing polyvinylidene fluoride, modified polyvinylidene fluoride, photosensitive oligomer, alumina, modified clay, initiator and dihydrolevorotatory glucosone; the coating of PVDF slurry firstly increases the mechanical properties and aging resistance of the aging-resistant PET film; secondly, it inhibits the degradation of the PET base film during use; thirdly, it can enhance the high temperature resistance of the aging-resistant PET film, thereby facilitating the deposition of a metal layer on its surface at a higher temperature and increasing the thermal stability of the aging-resistant PET film.

[0026] Among them, the modified polyvinylidene fluoride is based on polyvinylidene fluoride, which is first hydroxylated and then grafted with modified cyclodextrin and acrylic acid. The modification of cyclodextrin improves the porosity of the coating and can improve the electrolyte wettability, ion conductivity and thermal stability; in addition, the interface affinity with alumina and modified clay is increased, and the dispersibility of the filler is increased; in addition, the grafting of modified cyclodextrin and acrylic acid chain segments on the hydroxylated polyvinylidene fluoride makes it contain unsaturated bonds, thereby generating cross-linking under light, thereby promoting interface adhesion. Similarly, the introduction of photosensitive oligomers plays a role in toughening and cross-linking. It is a photosensitive polyurethane acrylate oligomer prepared from polyneopentyl adipate, 2,2,3,3-tetrafluoro-1,4-butanediol, diisocyanate, 1,3,5-cyclohexanetriol, and pentaerythritol triacrylate. The introduction of 1,3,5-cyclohexanetriol gives it a branched structure, thereby producing toughening; the introduction of 2,2,3,3-tetrafluoro-1,4-butanediol improves its affinity with polyvinylidene fluoride, and the introduction of pentaerythritol triacrylate increases its cross-linking with modified polyvinylidene fluoride, increases cohesion, and improves the interfacial adhesion of PVDF slurry. The modified clay is first modified by intercalation with hexadecyltrimethylammonium bromide and then modified with tetrabutyl titanate and lacquer phenol. The introduction of the modified substance can effectively improve the corrosion resistance of the coating, thereby improving the aging resistance; at the same time, the modified substance can increase the affinity with the electrolyte and improve the ion mobility, thereby improving the stability and electrical properties of the aging-resistant PET film when used in batteries.

[0027] In summary, by introducing modified polyvinylidene fluoride and photosensitive oligomers, the dispersibility of PVDF-reinforced alumina in PVDF slurry is increased, and the cross-linking property is increased; thereby, the interfacial adhesion between PVDF slurry and PET base film is enhanced, the aging of the interfacial adhesion during the recycling process is inhibited, the de-powdering property is inhibited, and the safety is increased; and further, modified clay is introduced to increase the electrolyte resistance of the aging-resistant PET film, thereby further improving the aging resistance and service life.

[0028] In the scheme, in order to further improve the applicability of the aging-resistant PET film in the current collector, PVDF-HFP slurry is further coated. Among them, the slurry contains (vinylidene fluoride-co-hexafluoropropylene) with good breakdown strength, which can improve safety, and at the same time increase the interface affinity between the aging-resistant PET film and the copper layer or aluminum layer, reduce the interface resistance, thereby improving the practical applicability of the aging-resistant PET film; in addition, modified polyvinylidene fluoride, dimethylaminoethyl methacrylate, and modified clay are introduced into the slurry to increase the affinity with the PVDF layer, interface crosslinking and aging resistance, thereby enhancing the service life of the aging-resistant PET film. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] It should be noted that the following parts are parts by mass; the purchase manufacturers of all raw materials involved in the present invention are exemplified without any special restrictions: in the following embodiments, the CAS number of β-cyclodextrin is 7585-39-9; the CAS number of N,N'-carbonyldiimidazole is 530-62-1; the CAS number of 1-amino-2-vinylcyclopropanecarboxylic acid is 80003-54-9; the CAS number of potassium permanganate is 7722-64-7; the CAS number of potassium hydroxide is 1310-58-3; the CAS number of sodium bisulfite is 7631-90-5; the CAS number of acrylic acid is 79-10-7; the CAS number of 2,2,3,3-tetrafluoro-1,4-butanediol is 425-61-6; the CAS number of isophorone diisocyanate is 4098-71-9; the CAS number of pentaerythritol triacrylate is 3524-6 8-3; the CAS number of lacquer phenol is 83258-37-1; the CAS number of tetrabutyl titanate is 5593-70-4; the CAS number of hexadecyltrimethylammonium bromide is 57-09-0; the CAS number of dimethylaminoethyl methacrylate is 2867-47-2; the clay is nano-grade, with the product number 682659, provided by Sigma-Aldrich (Shanghai) Trading Co., Ltd.; the CAS number of dihydro-levulinone is 53716-82-8, provided by Jinan Shangbo Biotechnology Co., Ltd.; the model of polyvinylidene fluoride is HSV900, provided by Guangzhou Hongcheng Plastic Co., Ltd.; the model of poly(vinylidene fluoride-co-hexafluoropropylene) is Arkema LBG, provided by Suzhou Qinshang Fluoroplastic Co., Ltd.; the alumina is high-purity ultrafine alumina with an average particle size of about 450nm, provided by Qinghe County Ruijiang Metal Materials Co., Ltd.

[0031] In the following examples, the coating thickness of the PVDF slurry is 2 μm, and the coating thickness of the PVDF-HFP slurry is 1 μm. The preparation method of the PET base film is as follows: 100 parts of PET resin (PETCZ-333), 6 parts of aluminum oxide, 2 parts of KH-550 silane coupling agent, 1 part of ethylene bis stearamide, and 1 part of phosphite antioxidant (antioxidant MIANOX168) are mixed, melt-extruded at 220°C, stretched at 110°C with a transverse stretching ratio of 1:3 and a longitudinal stretching ratio of 1:4; and shaped to obtain a 3 μm PET base film.

[0032] Raw material preparation: (1) Preparation of modified polyvinylidene fluoride: S1: Add 10 parts of β-cyclodextrin to 100 parts of DMF, add 0.42 parts of N,N'-carbonyldiimidazole, stir at 20°C for 2 hours; add 0.34 parts of 1-amino-2-vinylcyclopropanecarboxylic acid, continue stirring and reacting for 24 hours to obtain modified cyclodextrin; S2: Add 30 parts of polyvinylidene fluoride to 60 parts of DMF, stir at 25°C for 2 hours, wash with water; transfer it to a mixed aqueous solution A containing potassium permanganate and potassium hydroxide (the content of potassium permanganate is 4.5wt%, and the content of potassium hydroxide is 4.5wt%). The potassium content is 20wt%), stirred at 0~25℃ for 8 hours, washed with water; transferred to a mixed aqueous solution B containing sulfuric acid and sodium bisulfite (the content of sulfuric acid is 5wt%, the content of sodium bisulfite is 5wt%), stirred at 25℃ for 2 hours, washed with water, and dried to obtain hydroxylated polyvinylidene fluoride; S3: 16.8 parts of acrylic acid are added to 7.5 parts of ethylene glycol, 20 parts of hydroxylated polyvinylidene fluoride, 5.7 parts of modified cyclodextrin, and 4.2 parts of 98% concentrated sulfuric acid are added; the temperature is raised to 90℃, stirred for reaction for 5 hours, washed with water, and dried to obtain modified polyvinylidene fluoride.

[0033] (2) Preparation of photosensitive oligomer: 17.5 parts of poly (neopentyl adipate) and 3 parts of 2,2,3,3-tetrafluoro-1,4-butanediol were mixed, vacuumized at 95°C and stirred for 60 minutes; the temperature was lowered to 70°C, 9.8 parts of isophorone diisocyanate and 0.015 parts of organotin T-12 were added, and the temperature was raised to 90°C for reaction. When the -NCO content reached 8.6%, 13 parts of 1,3,5-cyclohexanetriol were added, and the reaction was continued until the -NCO content reached 3%. 7.8 parts of pentaerythritol triacrylate were added, and the reaction was continued for 2.5 hours to obtain a photosensitive oligomer.

[0034] (3) Preparation of modified clay: ultrasonically disperse 10 parts of clay in 100 parts of ethanol-water solution (the mass ratio of ethanol to water is 1:1), add 3.2 parts of hexadecyltrimethylammonium bromide and ultrasonically disperse it again, then heat it to 80°C, stir for 5 hours, filter, wash with water, and freeze-dry to obtain powder; add 10 parts of powder and 4.1 parts of tetrabutyl titanate to 50 parts of xylene in turn, stir at room temperature for 2-3 hours, add a xylene solution containing urushiol (7.3 parts of urushiol, 50 parts of xylene), heat to 85°C for reaction for 1 hour, then heat to 120°C for stirring for 2 hours, continue to heat to 130°C for stirring for 1 hour, cool, wash with water, and dry to obtain modified clay.

[0035] Embodiment 1: A method for preparing an aging-resistant PET film, comprising the following steps:

[0036] Step 1: 2 parts of polyvinylidene fluoride, 3.5 parts of modified polyvinylidene fluoride, 7.5 parts of photosensitive oligomer, 32 parts of aluminum oxide, 10 parts of modified clay, and 0.15 parts of initiator 184 are sequentially added to 120 parts of dihydro-levulinic ketone, and homogenized to obtain PVDF slurry;

[0037] Step 2: 20 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 8 parts of modified polyvinylidene fluoride, 5 parts of dimethylaminoethyl methacrylate, 3 parts of modified clay, 9 parts of water-based additives (3 parts of BYK-LPC22136, 2 parts of BYK-1785, 4 parts of LAPONITE-RD), and 0.1 parts of initiator 184 were sequentially added to 120 parts of deionized water, and homogenized to obtain PVDF-HFP slurry;

[0038] Step 3: First coat the surface of the PET base film with PVDF slurry at a coating speed of 30 m / min and a coating tension of 20 N, place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 10 seconds; then coat the PVDF-HFP slurry at a coating speed of 15 m / min and a coating tension of 20 N, again place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 25 seconds; then place the film in deionized water, undergo eight-stage extraction to remove dihydro-L-glucose ketone; dry at 80°C to obtain an aging-resistant PET film.

[0039] Embodiment 2: A method for preparing an aging-resistant PET film, comprising the following steps:

[0040] Step 1: 2 parts of polyvinylidene fluoride, 4 parts of modified polyvinylidene fluoride, 5 parts of photosensitive oligomer, 32 parts of alumina, 10 parts of modified clay, and 0.15 parts of initiator 184 are sequentially added to 100 parts of dihydro-levulinic ketone, and homogenized to obtain PVDF slurry;

[0041] Step 2: 20 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 8 parts of modified polyvinylidene fluoride, 4 parts of dimethylaminoethyl methacrylate, 2 parts of modified clay, 8 parts of water-based additives (2 parts of BYK-LPC22136, 2 parts of BYK-1785, 4 parts of LAPONITE-RD), and 0.1 parts of initiator 184 were sequentially added to 100 parts of deionized water, and homogenized to obtain PVDF-HFP slurry;

[0042] Step 3: First coat the surface of the PET base film with PVDF slurry at a coating speed of 30 m / min and a coating tension of 20 N, place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 10 seconds; then coat the PVDF-HFP slurry at a coating speed of 15 m / min and a coating tension of 20 N, again place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 25 seconds; then place the film in deionized water, undergo eight-stage extraction to remove dihydro-L-glucose ketone; dry at 80°C to obtain an aging-resistant PET film.

[0043] Embodiment 3: A method for preparing an aging-resistant PET film, comprising the following steps:

[0044] Step 1: 3 parts of polyvinylidene fluoride, 3 parts of modified polyvinylidene fluoride, 8 parts of photosensitive oligomer, 40 parts of alumina, 8 parts of modified clay, and 0.15 parts of initiator 184 are sequentially added to 120 parts of dihydro-levulinic ketone, and homogenized to obtain PVDF slurry;

[0045] Step 2: 22 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 5 parts of modified polyvinylidene fluoride, 6 parts of dimethylaminoethyl methacrylate, 2 parts of modified clay, 10 parts of water-based additives (3 parts of BYK-LPC22136, 2 parts of BYK-1785, 5 parts of LAPONITE-RD), and 0.1 parts of initiator 184 were sequentially added to 120 parts of deionized water, and homogenized to obtain PVDF-HFP slurry;

[0046] Step 3: First coat the surface of the PET base film with PVDF slurry at a coating speed of 30 m / min and a coating tension of 20 N, place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 10 seconds; then coat the PVDF-HFP slurry at a coating speed of 15 m / min and a coating tension of 20 N, again place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 25 seconds; then place the film in deionized water, undergo eight-stage extraction to remove dihydro-L-glucose ketone; dry at 80°C to obtain an aging-resistant PET film.

[0047] Comparative Example 1: PVDF slurry and PVDF-HFP slurry do not introduce modified polyvinylidene fluoride, and the rest is the same as Example 1; comprising the following steps:

[0048] Step 1: 5.5 parts of polyvinylidene fluoride, 7.5 parts of photosensitive oligomer, 32 parts of aluminum oxide, 10 parts of modified clay, and 0.15 parts of initiator 184 are sequentially added to 120 parts of dihydro-levulinic ketone, and homogenized to obtain PVDF slurry;

[0049] Step 2: 28 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 5 parts of dimethylaminoethyl methacrylate, 3 parts of modified clay, 9 parts of water-based additives (3 parts of BYK-LPC22136, 2 parts of BYK-1785, 4 parts of LAPONITE-RD), and 0.1 parts of initiator 184 were sequentially added to 120 parts of deionized water, and homogenized to obtain PVDF-HFP slurry;

[0050] Step 3: First coat the surface of the PET base film with PVDF slurry at a coating speed of 30 m / min and a coating tension of 20 N, place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 10 seconds; then coat the PVDF-HFP slurry at a coating speed of 15 m / min and a coating tension of 20 N, again place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 25 seconds; then place the film in deionized water, undergo eight-stage extraction to remove dihydro-L-glucose ketone; dry at 80°C to obtain an aging-resistant PET film.

[0051] Comparative Example 2: The modified clay is replaced by alumina, and the rest is the same as Example 1; comprising the following steps:

[0052] Step 1: 2 parts of polyvinylidene fluoride, 3.5 parts of modified polyvinylidene fluoride, 7.5 parts of photosensitive oligomer, 42 parts of aluminum oxide, and 0.15 parts of initiator 184 are sequentially added to 120 parts of dihydro-levulinic ketone, and homogenized to obtain PVDF slurry;

[0053] Step 2: 20 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 8 parts of modified polyvinylidene fluoride, 5 parts of dimethylaminoethyl methacrylate, 3 parts of alumina, 9 parts of water-based additives (3 parts of BYK-LPC22136, 2 parts of BYK-1785, 4 parts of LAPONITE-RD), and 0.1 parts of initiator 184 were sequentially added to 120 parts of deionized water, and homogenized to obtain PVDF-HFP slurry;

[0054] Step 3: First coat the surface of the PET base film with PVDF slurry at a coating speed of 30 m / min and a coating tension of 20 N, place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 10 seconds; then coat the PVDF-HFP slurry at a coating speed of 15 m / min and a coating tension of 20 N, again place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 25 seconds; then place the film in deionized water, undergo eight-stage extraction to remove dihydro-L-glucose ketone; dry at 80°C to obtain an aging-resistant PET film.

[0055] Comparative Example 3: The modification method of the modified clay is different, and the rest is the same as Example 1; the specific different steps are as follows:

[0056] Preparation of modified clay: 10 parts of clay were ultrasonically dispersed in 100 parts of ethanol aqueous solution (the mass ratio of ethanol to water was 1:1), 3.2 parts of hexadecyltrimethylammonium bromide and 3 parts of 3-methacrylatepropyltri(trimethoxysilyl) were added and ultrasonically dispersed again, then heated to 80°C, stirred for 5 hours, filtered, washed with water, and freeze-dried to obtain modified clay.

[0057] Comparative Example 4: The photosensitive oligomer is replaced with polyethylene glycol diacrylate (CAS No. 26570-48-9, brand TCI), and the rest is the same as Example 1; comprising the following steps:

[0058] Step 1: 2 parts of polyvinylidene fluoride, 3.5 parts of modified polyvinylidene fluoride, 7.5 parts of polyethylene glycol diacrylate, 32 parts of alumina, 10 parts of modified clay, and 0.15 parts of initiator 184 are sequentially added to 120 parts of dihydro-levulinone, and homogenized to obtain PVDF slurry;

[0059] Step 2: 20 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 8 parts of modified polyvinylidene fluoride, 5 parts of dimethylaminoethyl methacrylate, 3 parts of modified clay, 9 parts of water-based additives (3 parts of BYK-LPC22136, 2 parts of BYK-1785, 4 parts of LAPONITE-RD), and 0.1 parts of initiator 184 were sequentially added to 120 parts of deionized water, and homogenized to obtain PVDF-HFP slurry;

[0060] Step 3: First coat the surface of the PET base film with PVDF slurry at a coating speed of 30 m / min and a coating tension of 20 N, place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 10 seconds; then coat the PVDF-HFP slurry at a coating speed of 15 m / min and a coating tension of 20 N, again place the film at a distance of 10 cm from a 1 kW UV lamp, and irradiate with UV light for 25 seconds; then place the film in deionized water, undergo eight-stage extraction to remove dihydro-L-glucose ketone; dry at 80°C to obtain an aging-resistant PET film.

[0061] Performance test: (1) The aging-resistant PET film was tested for tensile strength at a rate of 5 mm / min using an electronic universal mechanical testing machine in accordance with GB / T 1040.1-2018; it was aged in hot air at 100°C for 96 hours, the tensile strength was tested again, and the tensile strength retention rate was calculated; (2) 3M double-sided tape was attached to a stainless steel plate, the aging-resistant PET film was placed on the double-sided tape, rolled back and forth 5 times, and then placed on a tester to test the peel strength at a speed of 50 mm / min; ethylene carbonate, diethyl carbonate and methyl ethyl carbonate were mixed and homogenized in a mass ratio of 1:2:1 to obtain an electrolyte, the aging-resistant PET film was placed in the electrolyte, sealed, placed at 60°C for 15 days, taken out, the electrolyte was removed, the peel strength was tested again, and the peel strength retention rate was calculated. The obtained data are shown below:

[0062]

[0063] Conclusion: From the data in the above table, it can be seen that the present application has prepared an aging-resistant PET film for current collector with excellent mechanical properties and aging resistance, which has excellent stability in the electrolyte and effectively improves the practical applicability. From the data of Comparative Examples 1 to 4, it can be seen that in Comparative Example 1, the PVDF slurry and PVDF-HFP slurry do not introduce modified polyvinylidene fluoride, which reduces the interface performance, thereby reducing the aging resistance, especially in the electrolyte. The aging resistance of the peel strength has a significant effect. In Comparative Example 2, since the modified clay is replaced with alumina, the crosslinking degree and electrolyte resistance are reduced, resulting in a decrease in aging resistance; in Comparative Example 3, due to the different modification methods of the modified clay, the interface performance is reduced, resulting in a decrease in aging resistance; in Comparative Example 4, since the photosensitive oligomer is replaced with polyethylene glycol diacrylate, the crosslinking and toughening properties are reduced, resulting in a decrease in comprehensive performance.

[0064] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an aging-resistant PET film, characterized in that: The following steps are involved: Step 1: adding polyvinylidene fluoride, modified polyvinylidene fluoride, photosensitive oligomer, alumina, modified clay, and initiator to dihydro-levorotatory glucosone in sequence, and homogenizing to obtain PVDF slurry; Step 2: Add poly(vinylidene fluoride-co-hexafluoropropylene), modified polyvinylidene fluoride, dimethylaminoethyl methacrylate, modified clay, water-based additive, and initiator to deionized water in sequence, and homogenize to obtain PVDF-HFP slurry; Step 3: firstly coat the surface of the PET base film with PVDF slurry and irradiate with ultraviolet light for 10 to 15 seconds; then coat the PVDF-HFP slurry and irradiate with ultraviolet light for 20 to 30 seconds; then place the surface of the PET base film in deionized water for extraction and cleaning; and dry the surface at 60 to 80° C. to obtain an aging-resistant PET film; Preparation method of modified polyvinylidene fluoride The following steps are involved: S1: Add β-cyclodextrin to DMF, add N,N'-carbonyldiimidazole, and stir at 20-25°C for 2-3 hours; add 1-amino-2-vinylcyclopropanecarboxylic acid, continue stirring and reacting for 20-24 hours to obtain modified cyclodextrin; S2: Add polyvinylidene fluoride to DMF, stir at 20-25°C for 2-3 hours, and wash with water; Transfer it to a mixed aqueous solution A containing potassium permanganate and potassium hydroxide, stir at 20-25°C for 8-10 hours, and wash with water; transfer it to a mixed aqueous solution B containing sulfuric acid and sodium bisulfite, stir at 20-25°C for 2-3 hours, wash with water, and dry to obtain hydroxylated polyvinylidene fluoride; S3: add acrylic acid to ethylene glycol, add hydroxylated polyvinylidene fluoride, modified cyclodextrin, and concentrated sulfuric acid; heat to 90-95°C, stir and react for 4-6 hours, wash with water, and dry to obtain modified polyvinylidene fluoride; The preparation method of the photosensitive oligomer is as follows: poly (neopentyl adipate) glycol ester and 2,2,3,3-tetrafluoro-1,4-butanediol are mixed, and the mixture is stirred for 40 to 60 minutes after vacuuming at 95 to 100° C.; the mixture is cooled to 70 to 75° C., diisocyanate and organotin are added, and the mixture is heated to 85 to 90° C. for reaction, and when the -NCO content is 8 to 9%, 1,3,5-cyclohexanetriol is added, and the reaction is continued until the -NCO content is 2.5 to 3.5%, and pentaerythritol triacrylate is added, and the reaction is continued for 2 to 2.5 hours to obtain the photosensitive oligomer; The preparation method of the modified clay comprises the following steps: ultrasonically dispersing the clay in an ethanol aqueous solution, adding hexadecyltrimethylammonium bromide and ultrasonically dispersing it again, then heating it to 80-85°C, stirring it for 4-5 hours, filtering, washing with water, and freeze-drying it to obtain a powder; sequentially adding the powder and tetrabutyl titanate into xylene, stirring it at room temperature for 2-3 hours, adding a xylene solution containing urushiol, heating it to 80-85°C and reacting it for 1-1.5 hours, then heating it to 115-120°C and stirring it for 1-2 hours, then heating it to 125-135°C and stirring it for 0.5-1 hour, cooling it, washing with water, and drying it to obtain the modified clay.

2. The method for preparing an aging-resistant PET film according to claim 1, characterized in that: The PVDF slurry comprises the following components: by weight, 2-3 parts of polyvinylidene fluoride, 3-4 parts of modified polyvinylidene fluoride, 5-8 parts of photosensitive oligomer, 32-40 parts of aluminum oxide, 8-10 parts of modified clay, 0.1-0.2 parts of initiator, and 100-120 parts of dihydro-levulinone.

3. The method for preparing an aging-resistant PET film according to claim 1, characterized in that: The PVDF-HFP slurry comprises the following components: by weight: 20 to 22 parts of poly(vinylidene fluoride-co-hexafluoropropylene), 5 to 8 parts of modified polyvinylidene fluoride, 4 to 6 parts of dimethylaminoethyl methacrylate, 2 to 4 parts of modified clay, 8 to 10 parts of water-based additives, 0.1 to 0.2 parts of initiator, and 100 to 120 parts of deionized water.

4. The method for preparing an aging-resistant PET film according to claim 1, characterized in that: Among the raw materials of the modified cyclodextrin, the mass ratio of β-cyclodextrin, N,N'-carbonyldiimidazole, and 1-amino-2-vinylcyclopropanecarboxylic acid is 1:(0.4-0.43):(0.3-0.35); the raw materials of the modified polyvinylidene fluoride include the following components: by weight, 20 parts of hydroxylated polyvinylidene fluoride, 16-17 parts of acrylic acid, 7-8 parts of ethylene glycol, 5-6 parts of modified cyclodextrin, and 4-5 parts of concentrated sulfuric acid.

5. The method for preparing an aging-resistant PET film according to claim 1, characterized in that: In the mixed aqueous solution A, the content of potassium permanganate is 4-4.2wt%, and the content of potassium hydroxide is 19.8-20wt%; in the mixed aqueous solution B, the content of sulfuric acid is 4.5-5wt%, and the content of sodium bisulfite is 4.5-5wt%.

6. The method for preparing an aging-resistant PET film according to claim 1, characterized in that: The raw materials of the photosensitive oligomer include the following components: by weight, 16 to 18 parts of polyneopentyl adipate, 2 to 4 parts of 2,2,3,3-tetrafluoro-1,4-butanediol, 8 to 10 parts of diisocyanate, 0.01 to 0.02 parts of organic tin, 12 to 14 parts of 1,3,5-cyclohexanetriol, and 7 to 8 parts of pentaerythritol triacrylate.

7. The method for preparing an aging-resistant PET film according to claim 1, characterized in that: The mass ratio of clay to hexadecyltrimethylammonium bromide is 10:(2.5-3.5); the mass ratio of powder, tetrabutyl titanate and urushiol is 10:(4-4.2):(7-7.5).

8. The aging-resistant PET film prepared by the method for preparing an aging-resistant PET film according to any one of claims 1 to 7, characterized in that: The thickness of the PET base film is 3-6 μm; the coating thickness of the PVDF slurry is 2-3 μm, and the coating thickness of the PVDF-HFP slurry is 0.5-1 μm.