A magnetic roller wear-resistant coating and its spraying process
By using materials such as hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic modified polyetheretherketone, combined with fillers and cellulose nanocrystals, and using UV curing and high-voltage electrostatic spraying technology, the surface coating of the magnetic roller is solved In order to solve the problem of insufficient performance, it has improved corrosion resistance, moisture and heat aging resistance and wear resistance, simplified the process and reduced environmental impact.
Patent Information
- Application Number
- CN202410637516.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-22
AI Technical Summary
The wear resistance, adhesion, moisture and heat aging resistance and corrosion resistance of the existing magnetic roller surface coating are insufficient, and the spraying process has problems such as high equipment dependence and large environmental impact.
Using hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic modified polyetheretherketone as the main components, combined with fillers such as boron fiber and molybdenum disulfide, the coating is prepared through a UV curing process and used in the spraying process Using high-voltage electrostatic spraying technology, cellulose nanocrystals are added to improve the corrosion resistance and moisture-heat aging resistance of the coating.
It significantly improves the scrubbing resistance, impact resistance, adhesion and wear resistance of the magnetic roller coating, extends the service life, simplifies the process and reduces the impact on the environment.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a magnetic roller wear-resistant coating and a spraying process thereof. Background Art
[0002] In the process of mineral mining, the newly mined ore sand is often complex in composition and contains impurities of various properties. Especially when mining metal ores, some of the mixed ore sand is often screened out according to needs. The most common screening method is to screen out magnetic ore sand or non-magnetic ore sand according to the magnetic strength of different ore sands. In the existing technology, the screening of magnetic ore sand is usually achieved through a magnetic separator. The magnetic roller is one of the important components of the magnetic separator. It not only affects the working efficiency of the magnetic separator, but also determines the sorting index of the mineral. It is particularly important to develop a magnetic roller with comprehensive performance and long service life.
[0003] Friction and wear are one of the most important reasons for the damage of magnetic rollers. In order to reduce the damage caused by friction and wear, friction and wear researchers have developed various friction reduction and wear resistance methods. One of the more commonly used methods is to set a coating on the surface of the magnetic roller, which is the most direct way to protect the magnetic roller of the magnetic separator. However, the wear resistance of the existing magnetic roller surface coating needs to be further improved, its adhesion to the magnetic roller is limited, and its moisture and heat aging resistance and corrosion resistance need to be further improved.
[0004] In order to solve the above problems, a Chinese invention patent with application announcement number CN111286265A discloses a wear-resistant UV-curable magnetic roller coating and a preparation method thereof. The coating is composed of the following raw materials by weight: 8-18 parts of graphene, 0.2-1.2 parts of methyl silicone oil, 2-12 parts of organic silicone resin, 0.2-1 parts of organic modified polysiloxane acrylic leveling agent, 0.2-2.5 parts of fumed silica, 10-32 parts of polyurethane acrylate, 0.01-15 parts of hexanediol diacrylate, 1-8 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-16 parts of inositol hexaphosphate, 0.25-2.5 parts of titanate coupling agent, 5-15 parts of alicyclic epoxy resin and 10-18 parts of zinc powder. The coating is prepared by multi-step mixing and dispersion. The coating is conductive after UV curing and has sufficient hardness, excellent wear resistance and tensile strength. However, its resistance to wet and hot aging, scrubbing resistance and impact resistance still need to be further improved.
[0005] It can be seen that the development of a magnetic roller wear-resistant coating and its spraying process with good corrosion resistance and moisture-heat aging resistance, good washability and impact resistance, strong adhesion and excellent wear resistance meets market demand, has broad market value and application prospects, and is of great significance to promoting the development of the magnetic roller coating field. Summary of the invention
[0006] The main purpose of the present invention is to provide a magnetic roller wear-resistant coating with good corrosion resistance and moisture-heat aging resistance, good scrubbing resistance and impact resistance, strong adhesion and excellent wear resistance, and a spraying process thereof.
[0007] To achieve the above purpose, the present invention provides a magnetic roller wear-resistant coating, which is made of the following raw materials in parts by weight: 40-50 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 20-25 parts of acrylic acid-modified polyetheretherketone, 1-2 parts of photoinitiator, 10-20 parts of filler, 1-3 parts of coupling agent, 0.5-1 parts of leveling agent, 0.3-0.7 parts of defoaming agent, 4-6 parts of 2,6-pyridinedicarbonyl chloride, and 0.8-1.5 parts of catalyst. , 10-(4-vinylphenyl)-10H-phenoxazine 1-3 parts, 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione 2-4 parts, isopropenylboronic acid pinacol ester 1-3 parts, 2-[3-(2H-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate 2-4 parts, cellulose nanocrystals 5-8 parts.
[0008] Preferably, there is no special requirement for the source of the hyperbranched perfluoropolyether polyurethane acrylate oligomer. In one embodiment of the present invention, the hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482680B.
[0009] Preferably, there is no special requirement for the source of the acrylic acid-modified polyetheretherketone. In one embodiment of the present invention, the acrylic acid-modified polyetheretherketone is prepared according to the method of Example 1 of Chinese invention patent with authorization publication number CN109337019B.
[0010] Preferably, the photoinitiator is at least one of benzoin ethyl ether, benzoin isopropyl ether, diphenyl acetone, and 2,4-dihydroxybenzophenone.
[0011] Preferably, the filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of (1-3):2; the average diameter of the boron fiber is 3-9 μm and the length is 3-5 mm; the particle size of the molybdenum disulfide is 1200-1600 mesh.
[0012] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0013] Preferably, the leveling agent is at least one of German BYK leveling agent BYK-333 and silicone leveling agent HY-5030.
[0014] Preferably, the defoamer is at least one of defoamer AT-99 and defoamer D6800.
[0015] Preferably, the catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride in a mass ratio of (2-4):3.
[0016] Preferably, the cellulose nanocrystals have a length of 100-500 nm and a diameter of 20-100 nm, and are provided by Beijing Nanosyn Technology Co., Ltd.
[0017] Another object of the present invention is to provide a spraying process for the magnetic roller wear-resistant coating, comprising the following steps:
[0018] Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material;
[0019] Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating;
[0020] Step S3, spray the UV-curable powder coating onto the surface of the magnetic roller using high voltage electrostatic spraying, with an average coating thickness of 60-80 microns, and then treat at 180-190° C. for 20-30 minutes, and then place under a 1KW high pressure mercury lamp, irradiated for 4-6 seconds at a distance of 30 cm from the lamp source.
[0021] Preferably, the voltage of the high-voltage electrostatic spraying is 60-90KV.
[0022] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0023] (1) The spraying process of the magnetic roller wear-resistant coating disclosed in the present invention is simple and easy to operate and control, has low dependence on equipment, low labor intensity and environmental impact, fast coating curing speed, is suitable for continuous large-scale use, and has high promotion and application value.
[0024] (2) The wear-resistant coating of the magnetic roller disclosed in the present invention is made of the following raw materials in parts by weight: 40-50 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 20-25 parts of acrylic acid-modified polyetheretherketone, 1-2 parts of photoinitiator, 10-20 parts of filler, 1-3 parts of coupling agent, 0.5-1 parts of leveling agent, 0.3-0.7 parts of defoaming agent, 4-6 parts of 2,6-pyridinedicarbonyl chloride, 0.8-1.5 parts of catalyst, 10 -(4-vinylphenyl)-10H-phenoxazine 1-3 parts, 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione 2-4 parts, isopropenylboronic acid pinacol ester 1-3 parts, 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methylacrylate 2-4 parts, cellulose nanocrystals 5-8 parts. Through the mutual cooperation between the raw materials, the prepared coating has good corrosion resistance and resistance to wet and hot aging, good washing resistance and impact resistance, strong adhesion and excellent wear resistance. Hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone are used as the main film-forming substances, combining the performance advantages of the two. Through the rational design of the raw material component formula, hyperbranched perfluoropolyether polyurethane, polyetheretherketone, pyridine, phenoxazine, triazone, boric acid pinacol ester and benzotriazole structures are simultaneously introduced into the molecular structure of the coating. Under the multiple effects of electronic effect, steric effect and conjugation effect, these structures make the finished product have better corrosion resistance and resistance to moisture and heat aging, better washability and impact resistance, stronger adhesion and better wear resistance.
[0025] (3) The wear-resistant coating of the magnetic roller disclosed in the present invention is cured by ultraviolet light, has a faster curing speed, does not use volatile organic solvents, and has less impact on the environment; the addition of cellulose nanocrystals, in combination with other raw material components, can effectively improve the comprehensive performance of the coating and extend its service life. The filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of (1-3):2. The reasonable selection of the filler composition formula can effectively improve the mechanical properties and wear resistance of the coating. DETAILED DESCRIPTION
[0026] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations. Example 1
[0027] A magnetic roller wear-resistant coating is prepared from the following raw materials in parts by weight: 40 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 20 parts of acrylic acid-modified polyetheretherketone, 1 part of photoinitiator, 10 parts of filler, 1 part of coupling agent, 0.5 parts of leveling agent, 0.3 parts of defoamer, 4 parts of 2,6-pyridinedicarbonyl chloride, 0.8 parts of catalyst, 1 part of 10-(4-vinylphenyl)-10H-phenoxazine, 2 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1 part of isopropenylboronic acid pinacol ester, 2 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, and 5 parts of cellulose nanocrystals.
[0028] The hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482680B; the acrylic acid-modified polyetheretherketone is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN109337019B.
[0029] The photoinitiator is benzoin ethyl ether; the filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of 1:2; the average diameter of the boron fiber is 3 μm and the length is 3 mm; the particle size of the molybdenum disulfide is 1200 mesh; the coupling agent is silane coupling agent KH550; the leveling agent is German BYK leveling agent BYK-333; the defoaming agent is defoaming agent AT-99; the catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride in a mass ratio of 2:3; the cellulose nanocrystals have a length of 100 nm and a diameter of 20 nm, and are provided by Beijing Naxun Technology Co., Ltd.
[0030] A spraying process for the magnetic roller wear-resistant coating comprises the following steps:
[0031] Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material;
[0032] Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating;
[0033] Step S3, spray the UV-curable powder coating on the surface of the magnetic roller using high-voltage electrostatic spraying, with an average coating thickness of 70 microns, and then treat it at 180°C for 20 minutes, and then place it under a 1KW high-pressure mercury lamp, 30 cm away from the lamp source, for 4 seconds; the voltage of the high-voltage electrostatic spraying is 60KV. Example 2
[0034] A magnetic roller wear-resistant coating is prepared from the following raw materials in parts by weight: 43 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 21 parts of acrylic acid-modified polyetheretherketone, 1.2 parts of photoinitiator, 12 parts of filler, 1.5 parts of coupling agent, 0.6 parts of leveling agent, 0.4 parts of defoamer, 4.5 parts of 2,6-pyridinedicarbonyl chloride, 1 part of catalyst, 1.5 parts of 10-(4-vinylphenyl)-10H-phenoxazine, 2.5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1.5 parts of isopropenylboronic acid pinacol ester, 2.5 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, and 6 parts of cellulose nanocrystals.
[0035] The hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482680B; the acrylic acid-modified polyetheretherketone is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN109337019B.
[0036] The photoinitiator is benzoin isopropyl ether; the filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of 1.5:2; the average diameter of the boron fiber is 5 μm and the length is 3.5 mm; the particle size of the molybdenum disulfide is 1300 mesh; the coupling agent is silane coupling agent KH560; the leveling agent is silicone leveling agent HY-5030; the defoaming agent is defoaming agent D6800; the catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride in a mass ratio of 2.5:3; the cellulose nanocrystal has a length of 200 nm and a diameter of 40 nm, and is provided by Beijing Naxun Technology Co., Ltd.
[0037] A spraying process for the magnetic roller wear-resistant coating comprises the following steps:
[0038] Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material;
[0039] Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating;
[0040] Step S3, using high-voltage electrostatic spraying to coat the UV-curable powder coating on the surface of the magnetic roller, with an average coating thickness of 70 microns, and then treating at 183°C for 22 minutes, and then placing it under a 1KW high-pressure mercury lamp, 30 cm away from the lamp source, for 4.5 seconds; the voltage of the high-voltage electrostatic spraying is 70KV. Example 3
[0041] A magnetic roller wear-resistant coating is prepared from the following raw materials in parts by weight: 45 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 23 parts of acrylic acid-modified polyetheretherketone, 1.5 parts of photoinitiator, 15 parts of filler, 2 parts of coupling agent, 0.7 parts of leveling agent, 0.5 parts of defoamer, 5 parts of 2,6-pyridinedicarbonyl chloride, 1.2 parts of catalyst, 2 parts of 10-(4-vinylphenyl)-10H-phenoxazine, 3 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2 parts of isopropenylboronic acid pinacol ester, 3 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, and 6.5 parts of cellulose nanocrystals.
[0042] The hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482680B; the acrylic acid-modified polyetheretherketone is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN109337019B.
[0043] The photoinitiator is diphenylacetophenone; the filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of 2:2; the average diameter of the boron fiber is 6 μm and the length is 4 mm; the particle size of the molybdenum disulfide is 1400 mesh; the coupling agent is silane coupling agent KH570; the leveling agent is German BYK leveling agent BYK-333; the defoaming agent is defoaming agent AT-99; the catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride in a mass ratio of 3:3; the cellulose nanocrystals have a length of 300 nm and a diameter of 70 nm, and are provided by Beijing Naxun Technology Co., Ltd.
[0044] A spraying process for the magnetic roller wear-resistant coating comprises the following steps:
[0045] Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material;
[0046] Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating;
[0047] Step S3, using high-voltage electrostatic spraying to coat the UV-curable powder coating on the surface of the magnetic roller, with an average coating thickness of 70 microns, and then treating at 185°C for 25 minutes, and then placing it under a 1KW high-pressure mercury lamp, 30 cm away from the lamp source, for 5 seconds; the voltage of the high-voltage electrostatic spraying is 75KV. Example 4
[0048] A magnetic roller wear-resistant coating is prepared from the following raw materials in parts by weight: 48 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 24 parts of acrylic acid-modified polyetheretherketone, 1.8 parts of photoinitiator, 18 parts of filler, 2.5 parts of coupling agent, 0.9 part of leveling agent, 0.6 part of defoamer, 5.5 parts of 2,6-pyridinedicarbonyl chloride, 1.4 parts of catalyst, 2.5 parts of 10-(4-vinylphenyl)-10H-phenoxazine, 3.5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2.5 parts of isopropenylboronic acid pinacol ester, 3.5 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, and 7.5 parts of cellulose nanocrystals.
[0049] The hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482680B; the acrylic acid-modified polyetheretherketone is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN109337019B.
[0050] The photoinitiator is a mixture of benzoin ethyl ether, benzoin isopropyl ether, diphenyl acetone, and 2,4-dihydroxybenzophenone in a mass ratio of 1:2:3:2; the filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of 2.5:2; the average diameter of the boron fiber is 8 μm and the length is 4.5 mm; the particle size of the molybdenum disulfide is 1500 mesh; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 1:2:1 The leveling agent is a mixture of German BYK leveling agent BYK-333 and silicone leveling agent HY-5030 mixed in a mass ratio of 1:3; the defoamer is a mixture of defoamer AT-99 and defoamer D6800 mixed in a mass ratio of 3:5; the catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride mixed in a mass ratio of 3.5:3; the cellulose nanocrystal has a length of 400nm and a diameter of 90nm, and is provided by Beijing Naxun Technology Co., Ltd.
[0051] A spraying process for the magnetic roller wear-resistant coating comprises the following steps:
[0052] Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material;
[0053] Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating;
[0054] Step S3, using high-voltage electrostatic spraying to coat the UV-curable powder coating on the surface of the magnetic roller, with an average coating thickness of 70 microns, and then treating at 188°C for 28 minutes, and then placing it under a 1KW high-pressure mercury lamp, 30cm away from the lamp source, for 5.5 seconds; the voltage of the high-voltage electrostatic spraying is 85KV. Example 5
[0055] A magnetic roller wear-resistant coating is prepared from the following raw materials in parts by weight: 50 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 25 parts of acrylic acid-modified polyetheretherketone, 2 parts of photoinitiator, 20 parts of filler, 3 parts of coupling agent, 1 part of leveling agent, 0.7 parts of defoamer, 6 parts of 2,6-pyridinedicarbonyl chloride, 1.5 parts of catalyst, 3 parts of 10-(4-vinylphenyl)-10H-phenoxazine, 4 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 3 parts of isopropenylboronic acid pinacol ester, 4 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, and 8 parts of cellulose nanocrystals.
[0056] The hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482680B; the acrylic acid-modified polyetheretherketone is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN109337019B.
[0057] The photoinitiator is 2,4-dihydroxybenzophenone; the filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of 3:2; the average diameter of the boron fiber is 9 μm and the length is 5 mm; the particle size of the molybdenum disulfide is 1600 mesh; the coupling agent is silane coupling agent KH550; the leveling agent is German BYK leveling agent BYK-333; the defoaming agent is defoaming agent D6800; the catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride in a mass ratio of 4:3; the cellulose nanocrystal has a length of 500 nm and a diameter of 100 nm, and is provided by Beijing Naxun Technology Co., Ltd.
[0058] A spraying process for the magnetic roller wear-resistant coating comprises the following steps:
[0059] Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material;
[0060] Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating;
[0061] Step S3, using high-voltage electrostatic spraying to coat the UV-curable powder coating on the surface of the magnetic roller, with an average coating thickness of 70 microns, and then treating at 190° C. for 30 minutes, and then placing it under a 1KW high-pressure mercury lamp, irradiating it for 6 seconds at a distance of 30 cm from the lamp source; the voltage of the high-voltage electrostatic spraying is 90KV.
[0062] Comparative Example 1
[0063] The present invention provides a magnetic roller wear-resistant coating and a spraying process thereof, which are similar to Example 1, except that 10-(4-vinylphenyl)-10H-phenoxazine and 2,6-pyridinedicarbonyl chloride are not added.
[0064] Comparative Example 2
[0065] The present invention provides a magnetic roller wear-resistant coating and a spraying process thereof, which are similar to Example 1, except that isopropenyl boric acid pinacol ester and cellulose nanocrystals are not added.
[0066] The magnetic roller wear-resistant coating samples prepared in the above Examples 1-5 and Comparative Examples 1-2 were subjected to relevant performance tests. The test results are shown in Table 1. The test method is as follows:
[0067] (1) Wear resistance: Tested in accordance with GB / T 1768-2006.
[0068] (2) Adhesion grade: Tested in accordance with GB / T 9286-1998.
[0069] (3) Corrosion resistance: Refer to GB / T 1771-2007 for salt spray resistance test, the test time is 1200h. If the coating has no blistering, softening, no micropores, and no change in viscosity, the corrosion resistance passes, otherwise it fails.
[0070] (4) Resistance to moisture and heat aging: Place each product under the environmental conditions of 90°C and 90% relative humidity for 600 hours. After cooling to room temperature, observe the changes in the coating. If the coating has no blistering, softening, micropores, and no change in viscosity, the moisture and heat aging resistance has passed; otherwise, it has failed.
[0071] (5) Washability: Tested in accordance with GB / T9266-2009.
[0072] (6) Impact resistance: Tested in accordance with GB / T 1732-1993.
[0073] Table 1
[0074] project Washability (times) Abrasion resistance (weight loss, mg) Adhesion grade (grade) Salt spray resistance test 1200h Heat and humidity resistance Impact resistance (kg·cm) Example 1 15220 3.3 1 pass pass 142 Example 2 15350 2.7 1 pass pass 145 Example 3 15450 1.9 1 pass pass 147 Example 4 15620 1.4 1 pass pass 152 Example 5 15700 1.1 1 pass pass 153 Comparative Example 1 14800 30 2 Not passed Not passed 124 Comparative Example 2 15037 22 2 Not passed Not passed 135
[0075] As can be seen from Table 1, the magnetic roller wear-resistant coating disclosed in the embodiment of the present invention has better scrub resistance, wear resistance, adhesion, corrosion resistance, moisture and heat resistance and impact resistance than the comparative example product; the combined use of 10-(4-vinylphenyl)-10H-phenoxazine, 2,6-pyridinedicarbonyl chloride, isopropenylboronic acid pinacol ester and cellulose nanocrystals is beneficial to improving the above properties.
[0076] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A magnetic roller wear-resistant coating, characterized in that: The invention is prepared from the following raw materials in parts by weight: 40-50 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 20-25 parts of acrylic acid modified polyetheretherketone, 1-2 parts of photoinitiator, 10-20 parts of filler, 1-3 parts of coupling agent, 0.5-1 parts of leveling agent, 0.3-0.7 parts of defoamer, 4-6 parts of 2,6-pyridine dicarbonyl chloride, 0.8-1.5 parts of catalyst, 10-(4-vinylbenzene The invention discloses a novel nanostructured carbonyl carbonate (C-type carbonyl carbonate) prepared from the following materials: 1-3 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1-3 parts of isopropenylboronic acid pinacol ester, 2-4 parts of 2-[3-(2H-benzotriazole-2-yl)-4-hydroxyphenyl]ethyl 2-methacrylate, and 5-8 parts of cellulose nanocrystals.
2. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The photoinitiator is at least one of benzoin ethyl ether, benzoin isopropyl ether, diphenyl acetone, and 2,4-dihydroxybenzophenone.
3. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The filler is a mixture of boron fiber and molybdenum disulfide in a mass ratio of (1-3):2; the average diameter of the boron fiber is 3-9 μm and the length is 3-5 mm; the particle size of the molybdenum disulfide is 1200-1600 mesh.
4. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570.
5. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The leveling agent is at least one of German BYK leveling agent BYK-333 and silicone leveling agent HY-5030.
6. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The defoamer is at least one of defoamer AT-99 and defoamer D6800.
7. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The catalyst is a mixture of anhydrous ferric chloride and anhydrous zinc chloride in a mass ratio of (2-4):
3.
8. The magnetic roller wear-resistant coating according to claim 1, characterized in that: The length of the cellulose nanocrystal is 100-500nm and the diameter is 20-100nm.
9. A spraying process for the wear-resistant coating of a magnetic roller according to any one of claims 1 to 8, characterized in that: The steps include: Step S1, firstly coarsely crushing the hyperbranched perfluoropolyether polyurethane acrylate oligomer and acrylic acid-modified polyetheretherketone, and then uniformly mixing them with other raw materials according to weight parts to obtain a mixed material; Step S2, extruding through a twin-screw extruder dedicated for powder coatings, and then cooling, crushing, micro-grinding, and screening to obtain a UV-curable powder coating; Step S3, spray the UV-curable powder coating onto the surface of the magnetic roller using high voltage electrostatic spraying, with an average coating thickness of 60-80 microns, and then treat at 180-190° C. for 20-30 minutes, and then place under a 1KW high-pressure mercury lamp, 30 cm away from the lamp source, for 4-6 seconds.
10. The spraying process of the magnetic roller wear-resistant coating according to claim 9 is characterized in that: The voltage of the high-voltage electrostatic spraying is 60-90KV.