A low temperature calcination process for ultrafine niobium oxide
Through low-temperature calcination process and air atmosphere treatment, the problem of agglomeration of ultrafine niobium oxide during calcination is solved, and ultrafine niobium oxide powder with smaller particle size and more uniform distribution is obtained, which improves the purity and uniformity of the product.
Patent Information
- Application Number
- CN202410592327.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-05-14
AI Technical Summary
Existing ultrafine niobium oxides are prone to agglomeration during the calcination process, resulting in excessive particles and uneven particle size distribution.
Using a low-temperature calcination process, including low-temperature fluorine calcination and further air atmosphere calcination, by mixing niobium hydroxide precursors with different particle sizes and controlling the calcination temperature and time, the grain growth rate of niobium oxide is regulated, avoiding agglomeration, and in the air atmosphere further remove impurities.
Effective regulation of particle size is achieved, and a smaller ultrafine niobium oxide powder with a more uniform particle size distribution is obtained, which improves the purity and particle size uniformity of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of powder metallurgy, and more specifically, relates to a low-temperature calcination process for ultrafine niobium oxide. Background Art
[0002] As an important electronic material, niobium pentoxide has been widely used in ceramic capacitors, piezoelectric ceramics, thick film capacitors, dielectric materials, magnetic materials, and optical materials. Adding niobium pentoxide can greatly improve the thermal stability of capacitors and obtain a stable and high dielectric constant. In recent years, due to the rapid development of liquid crystal displays, metal oxide targets have also received much attention and have developed rapidly.
[0003] Whether used as electronic materials or niobium oxide targets, ultrafine niobium oxide powder is required as raw material. Ultrafine niobium oxide powder is usually prepared by liquid phase reaction. In the liquid phase reaction, by strengthening the mixing intensity of the raw materials, the supersaturation of the precipitation product can be increased, which is conducive to the generation of powder particles with smaller particle size.
[0004] On the basis of the precursor obtained by liquid phase reaction, further drying and calcination are required. In this process, the selection of a suitable calcination process has a significant impact on the physical properties of the product. If the control is not good, it is easy to cause the particles to agglomerate or grow too much, resulting in the product particles not only having a large particle size, but also having an uneven particle size distribution. Based on this, how to control the preparation process to ensure that the product particles are small while maintaining a good uniformity is one of the technical problems faced by those skilled in the art. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the problem that the existing ultrafine niobium oxide is prone to agglomeration during the calcination process, resulting in excessively large particles, a narrow particle size distribution range, and uneven particle size, and provide a low-temperature calcination process for ultrafine niobium oxide.
[0006] The purpose of the present invention is to provide a low-temperature calcination process for ultrafine niobium oxide.
[0007] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0008] A low-temperature calcination process for ultrafine niobium oxide, the specific calcination process comprising:
[0009] Raw materials preparation:
[0010] After drying the niobium hydroxide, the niobium hydroxide is passed through a 60-mesh sieve to obtain pretreated niobium hydroxide;
[0011] Low temperature fluorine removal:
[0012] Dredging fluorine from the pretreated niobium hydroxide at low temperature to obtain a pretreated calcined material;
[0013] The low-temperature fluorine removal comprises: continuously calcining for 15-16 hours at a temperature of 400-450°C;
[0014] Continuous calcination:
[0015] The pre-treated calcined material is then heated to 600-650°C, calcined continuously, and then discharged to obtain ultrafine niobium oxide.
[0016] In the above calcination process, firstly, low-temperature fluorine removal is carried out. This is because, generally, the precursor of niobium hydroxide is prone to contain fluorine-containing impurities. In the process of low-temperature calcination, these impurities can be decomposed and removed, thereby avoiding their presence affecting the purity of the product. In addition, a composite precursor is prepared by mixing two niobium hydroxides with different D50. Therefore, in the low-temperature calcination process, the decomposition rates of precursors with different particle sizes will be different during the calcination process, thereby regulating the grain growth rate of niobium oxide to avoid excessive growth and agglomeration; in particular, under this temperature condition, niobium hydroxide particles with smaller particle sizes are preferentially decomposed, while those with relatively larger particle sizes are decomposed more slowly, so that the particle size of the final product can be effectively regulated.
[0017] Furthermore, in the specific calcination process,
[0018] The low-temperature fluorine removal also includes: removing fluorine from the composite precursor at a temperature of 400-410° C. to obtain a pretreated calcined material;
[0019] The continuous calcination further comprises: in an air atmosphere, heating the pretreated calcined material to 640-650° C., continuing to calcine for 20-24 hours, and then discharging the material to obtain ultrafine niobium oxide.
[0020] By further calcining in an air atmosphere, the grain growth can be further regulated during this process, and impurities therein can be removed, so that the purity of the product can be guaranteed.
[0021] Furthermore, the niobium hydroxide includes a first niobium hydroxide and a second niobium hydroxide, the D50 of the first niobium hydroxide is 10-30 nm, and the D50 of the second niobium hydroxide is 45-50 nm.
[0022] A composite precursor is prepared by mixing two niobium hydroxides with different D50s. Thus, during the low-temperature calcination process, the decomposition rates of the precursors with different particle sizes will be different during the calcination process, so that the grain growth rate of niobium oxide can be regulated to avoid excessive growth and agglomeration; in particular, under this temperature condition, the niobium hydroxide particles with smaller particle sizes decompose first, while the particles with relatively larger particle sizes decompose more slowly, so that the particle size of the final product can be effectively regulated.
[0023] Furthermore, the low-temperature fluorine removal also includes:
[0024] The composite precursor is first calcined at a temperature of 280-330° C. for 4-6 hours, and then the temperature is raised to 400-410° C. and calcined for 15-16 hours. DETAILED DESCRIPTION
[0025] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0026] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0027] Example 1
[0028] Raw materials preparation:
[0029] After drying the niobium hydroxide, the niobium hydroxide is passed through a 60-mesh sieve to obtain pretreated niobium hydroxide;
[0030] The niobium hydroxide includes a first niobium hydroxide and a second niobium hydroxide, the D50 of the first niobium hydroxide is 10 nm, the D50 of the second niobium hydroxide is 45 nm, and the D50 of the porous carbon is 200 μm;
[0031] Low temperature fluorine removal:
[0032] Driving out fluorine from the composite precursor at low temperature to obtain a pre-treated calcined material;
[0033] The low-temperature fluorine removal comprises: firstly heating the composite precursor to 280°C at a rate of 3°C / min, calcining the composite precursor at 280°C for 4 hours, and then heating the composite precursor to 400°C at a rate of 4°C / min, and calcining the composite precursor for 15 hours to obtain a pre-treated calcined material;
[0034] Continuous calcination:
[0035] After the low-temperature fluorine removal is completed, continue heating at a rate of 6°C / min to 640°C. Continue calcining in an air atmosphere for 20 hours, then stop heating, cool to room temperature with the furnace, and discharge the material to obtain ultrafine niobium oxide.
[0036] Example 2
[0037] Raw materials preparation:
[0038] After drying the niobium hydroxide, the niobium hydroxide is passed through a 60-mesh sieve to obtain pretreated niobium hydroxide;
[0039] The niobium hydroxide includes a first niobium hydroxide and a second niobium hydroxide, the D50 of the first niobium hydroxide is 15 nm, the D50 of the second niobium hydroxide is 46 nm, and the D50 of the porous carbon is 280 μm;
[0040] Low temperature fluorine removal:
[0041] Driving out fluorine from the composite precursor at low temperature to obtain a pre-treated calcined material;
[0042] The low-temperature fluorine removal comprises: first heating to 300°C at a rate of 4°C / min, calcining the composite precursor at 300°C for 5 hours, and then heating to 405°C at a rate of 5°C / min, and calcining for 15 hours to obtain a pretreated calcined material;
[0043] Continuous calcination:
[0044] After the low-temperature fluorine removal is completed, continue heating at a rate of 7°C / min to 645°C. Continue calcining in an air atmosphere for 22 hours, then stop heating, cool to room temperature with the furnace, and discharge the material to obtain ultrafine niobium oxide.
[0045] Example 3
[0046] Raw materials preparation:
[0047] After drying the niobium hydroxide, the niobium hydroxide is passed through a 60-mesh sieve to obtain pretreated niobium hydroxide;
[0048] The niobium hydroxide includes a first niobium hydroxide and a second niobium hydroxide, the D50 of the first niobium hydroxide is 30 nm, the D50 of the second niobium hydroxide is 50 nm, and the D50 of the porous carbon is 400 μm;
[0049] Low temperature fluorine removal:
[0050] Driving out fluorine from the composite precursor at low temperature to obtain a pre-treated calcined material;
[0051] The low-temperature fluorine removal comprises: first heating to 330°C at a rate of 5°C / min, calcining the composite precursor at 330°C for 6 hours, and then heating to 410°C at a rate of 6°C / min, and calcining for 16 hours to obtain a pre-treated calcined material;
[0052] Continuous calcination:
[0053] After the low-temperature fluorine removal is completed, continue heating at a rate of 8°C / min to 650°C, continue calcining in an air atmosphere for 24 hours, stop heating, cool to room temperature with the furnace, and discharge the material to obtain ultrafine niobium oxide.
[0054] Comparative Example 1
[0055] The difference between this comparative example and Example 1 is that the second niobium hydroxide is not added, and the other conditions remain unchanged.
[0056] Specifically, raw material preparation:
[0057] After drying the niobium hydroxide, the niobium hydroxide is passed through a 60-mesh sieve to obtain pretreated niobium hydroxide;
[0058] The D50 of the niobium hydroxide is 10 nm;
[0059] Low temperature fluorine removal:
[0060] Driving out fluorine from the composite precursor at low temperature to obtain a pre-treated calcined material;
[0061] The low-temperature fluorine removal comprises: first heating to 280°C at a rate of 3°C / min under nitrogen atmosphere protection, calcining the composite precursor at 280°C for 4 hours, and then heating to 400°C at a rate of 4°C / min, and calcining for 15 hours to obtain a pretreated calcined material;
[0062] Continuous calcination:
[0063] After the low-temperature fluorine removal is completed, continue heating at a rate of 6°C / min to 640°C. Continue calcining in an air atmosphere for 20 hours, then stop heating, cool to room temperature with the furnace, and discharge the material to obtain ultrafine niobium oxide.
[0064] The performance of the products obtained in Examples 1-3 and Comparative Example 1 was tested, and the specific testing methods and test results are as follows:
[0065] The D50 and particle size distribution range of the product were tested using a laser particle size analyzer. The specific test results are shown in Table 1:
[0066] Table 1: Product performance test results
[0067]
[0068] It can be seen from the test results in Table 1 that the ultrafine niobium oxide product obtained in the present invention not only has a smaller particle size, but also has a narrower particle size distribution range and a more uniform size.
[0069] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A low temperature calcination process for ultrafine niobium oxide, characterized in that: The specific calcination process includes: Raw materials preparation: After drying the niobium hydroxide, the niobium hydroxide is passed through a 60-mesh sieve to obtain pretreated niobium hydroxide; The niobium hydroxide comprises a first niobium hydroxide and a second niobium hydroxide, wherein the D50 of the first niobium hydroxide is 10-30 nm, and the D50 of the second niobium hydroxide is 45-50 nm; Low temperature fluorine removal: Dredging fluorine from the pretreated niobium hydroxide at low temperature to obtain a pretreated calcined material; The low-temperature fluorine removal comprises: continuously calcining for 15-16 hours at a temperature of 400-450°C; Continue calcining: The pre-treated calcined material is then heated to 600-650°C, calcined continuously, and then discharged to obtain ultrafine niobium oxide.
2. The low temperature calcination process of ultrafine niobium oxide according to claim 1, characterized in that: In the specific calcination process, The low-temperature fluorine removal comprises: removing fluorine from the composite precursor at a temperature of 400-410° C. to obtain a pretreated calcined material; The further calcination comprises: in an air atmosphere, heating the pre-treated calcined material to 640-650° C., continuing calcination for 20-24 hours, and then discharging the material to obtain ultrafine niobium oxide.
3. The low temperature calcination process of ultrafine niobium oxide according to claim 1, characterized in that: The low-temperature fluorine removal comprises: First, the composite precursor is calcined at a temperature of 280-330° C. for 4-6 hours, and then the temperature is raised to 400-410° C. and calcined for 15-16 hours.