A kind of heat-resistant heat-insulating material and its application
Through the reaction of 3-(azidopropyl)silane with carboxyl-containing resin and the combination of inorganic fillers, a solid-gas-solid structure is formed, which solves the problem of burning and collapse of existing expanded microspheres at high temperatures, and achieves high-temperature isolation Thermal and flame retardant properties are suitable for thermal insulation applications under high temperature conditions.
Patent Information
- Application Number
- CN202410414923.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-08
AI Technical Summary
Existing expanded microsphere thermal insulation materials burn and collapse under high temperature conditions, which cannot meet the high temperature thermal insulation needs.
3-(azidopropyl)silane reacts with a carboxyl-containing resin at above 150°C to form an amine group-containing resin and release carbon dioxide and nitrogen to form a solid-gas-solid structure, combining inorganic fillers and flame retardants. Form a heat-resistant insulation material.
It achieves excellent thermal insulation effect and flame retardant properties of the material at high temperatures of 1300℃, and is suitable for thermal insulation applications under high temperature conditions.
Smart Images

Figure BDA0004780500600000011 
Figure BDA0004780500600000021 
Figure BDA0004780500600000022
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal insulation materials, and relates to a temperature-resistant thermal insulation material and application thereof; in particular, the material has excellent flame retardancy, heat insulation and high temperature resistance capabilities after being cured, and the temperature resistance of the material can reach 1300°C. Background Art
[0002] Currently, the self-expanding insulation materials on the market, such as expandable microspheres, are generally composed of liquid alkane gas sealed in a thermoplastic polymer. These expandable microspheres are hollow in the middle, and the average diameter ranges from 10 to 100μm. When the expandable microspheres are heated, the gas pressure in the shell increases and the thermoplastic polymer shell softens, causing the volume of the expandable microspheres to increase significantly. When cooled, the expandable microsphere polymer shell hardens again, making the polymer body fixed. After full expansion, the diameter and volume of the expandable microspheres will change. For example, the diameter increases from 20um to 40μm, and the volume increases by 2. 3 = 8 times. The common expansion temperature range is from 100 to 220℃. So after the expansion microspheres are added to the coating material, heating will cause the coating material to expand and form a central control polymer material filled with countless bubbles. This solid-gas-solid alternating material has low thermal conductivity and good thermal insulation effect.
[0003] However, since the expanded microspheres are filled with organic alkane gas, they will burn and collapse when exposed to high temperatures (such as 1300°C), so they cannot be used for thermal insulation under high temperature conditions. Summary of the invention
[0004] In view of the fact that existing coating products cannot meet the requirements, the purpose of the present invention is to provide a heat-resistant heat-insulating material and its application; the material is coated on the substrate to be protected, and solidified to form an expanded hollow heat-resistant heat-insulating material. In addition, the material can withstand a high temperature of 1300°C for a long time and has a good heat-insulating effect.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] The present invention relates to a heat-resistant and heat-insulating material, which comprises the following components in terms of weight percentage of the total weight of the material:
[0007]
[0008]
[0009] The amount of other organic solvents was made up to 100%.
[0010] As an embodiment of the present invention, the 3-(azidopropyl)silane can be 3-(azidopropyl)triethoxysilane, 3-(azidopropyl)trimethoxysilane or a mixture of the two. It can react with a carboxyl-containing resin at a temperature of 150° C. or above under the combined catalysis of palladium acetate (Pd(O2Ac)2) and DMAP to generate a larger molecular weight amine-containing resin and release carbon dioxide and nitrogen; the process is schematically shown as follows:
[0011]
[0012] The gas generation reaction is slower than the film curing reaction, that is, the gas is gradually generated after the film has been formed, and the generated carbon dioxide and nitrogen form pores of different sizes inside the material, thus forming an internal structure of solid-gas-solid, thereby achieving the effect of reducing the thermal conductivity of the material and heat insulation. In addition, these two gases are non-flammable and have flame retardant properties. In terms of mass percentage, the proportion of the total weight is 1-10%. Preferably, the proportion of 3-(azidopropyl)silane to the total weight is 2-5%.
[0013] In the system of the present invention, the flexible silicone resin containing carboxyl functional groups gradually self-crosslinks or reacts with the siloxy groups contained in 3-(azidopropyl) silane to form a film at 150°C, and the viscosity increases, locking the generated carbon dioxide and nitrogen inside the material. The molar equivalent of its carboxyl group and the molar equivalent of the azide group of 3-(azidopropyl) triethoxysilane are 2:1-1.1:1. If the molar ratio is too high, a large amount of carboxyl groups will remain, and too much residual carboxyl groups will cause the water resistance of the material itself to deteriorate. If the molar ratio is too low, the azide of 3-(azidopropyl) triethoxysilane will remain, which is dangerous.
[0014] As an embodiment of the present invention, the flexible silicone resin containing carboxyl functional groups is a carboxyl-terminated flexible silicone resin; specifically, a flexible heat-resistant silicone resin having carboxyl functional groups capped. Carboxyl functional group capping, that is, carboxyl groups are on both sides of the flexible resin, has little effect on the decrease of flexibility.
[0015] As one embodiment of the present invention, palladium acetate (Pd(O2Ac)2) is a catalyst, and its mass ratio to 3-(azidopropyl)silane is 1-5%. If the catalyst content is too low, the reaction rate will be affected, resulting in insufficient gas generation. If the catalyst content is too high, the gas generation rate will be too fast, and the material itself has not yet solidified into a film, and the gas has been produced, and finally other materials escape.
[0016] As an embodiment of the present invention, the inorganic filler is a solid inorganic filler, and its D50 particle size is 1nm-100μm. There is no special requirement for its particle size, but it must be a high temperature resistant (1300℃) inorganic filler, that is, a solid inorganic filler that is stable at 1300℃. Such as silicon dioxide, kaolin, silica, etc., which is mainly used to reduce costs and can be added or not.
[0017] As an embodiment of the present invention, the amount of the inorganic filler is 0.1-50%, and can be 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.
[0018] As an embodiment of the present invention, the 4-dimethylaminopyridine can be of industrial purity or above, and is also a catalyst, which cooperates with palladium acetate to catalyze the reaction shown in the following formula: The mass ratio of 4-dimethylaminopyridine to 3-(azidopropyl)silane is 1-5%.
[0019]
[0020] As an embodiment of the present invention, the flame retardant is a liquid or solid flame retardant, without specific restrictions. Since the material itself has non-flammable properties, the flame retardant may not be added, or it may be added to enhance the flame retardancy of the material. When adding the flame retardant, the amount thereof is selected to be 0.1-5%.
[0021] As an embodiment of the present invention, the other additives are one or more combinations of dispersants, defoamers, wetting and leveling agents, and rheological additives.
[0022] As an embodiment of the present invention, the dosage of the other auxiliary agents is 0.1-10%.
[0023] As an embodiment of the present invention, the high boiling point alcohol solvent can be one or more combinations of polyethylene glycol, polypropylene glycol, and dipropylene glycol.
[0024] As an embodiment of the present invention, the other organic solvents include one or more combinations of esters, ketones, alkane solvents, and aromatic solvents.
[0025] The present invention also relates to the application of a new temperature-resistant and heat-insulating material in preparation, which is sprayed, dipped or brushed on a substrate to be protected to form a coating material.
[0026] As an embodiment of the present invention, after the spraying, dipping or brushing, the coating is dried at 150-200° C. for 10-30 minutes to completely cure into a film.
[0027] As an embodiment of the present invention, the substrate includes steel, stainless steel, aluminum and electroplated substrates.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) It has high temperature resistance that existing products do not have, which makes it suitable for use in high temperature insulation fields.
[0030] 2) It has flame retardancy that existing products do not have, which makes it possible to be used for thermal insulation with open flames. DETAILED DESCRIPTION
[0031] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0032] The invention relates to a new temperature-resistant and heat-insulating material and application thereof.
[0033] In addition, in each embodiment, the preparation of the new heat-resistant and heat-insulating material is as follows: the components of the new heat-resistant and heat-insulating material are physically mixed and then dispersed at high speed until the mixture is uniformly mixed, which can be used for performance testing.
[0034] Preparation of test panels: Unless otherwise specified, the test panels are Q-panel cold-rolled steel panels. The test panels are degreased and cleaned with a degreaser and dried for use. The materials are applied to the pre-treated test panels by air spraying. After curing, the relevant properties are tested. Adhesion tests are performed in accordance with GB / T 9286-1998. Thermal conductivity is tested in accordance with ASTM D5470.
[0035] Embodiment 1, 2
[0036] The present embodiments 1 and 2 relate to a heat-resistant and heat-insulating material, the composition and mass dosage of which are shown in Table 1:
[0037] Table 1
[0038]
[0039] Remark: 1 Purchased from Shanghai Aladdin Reagent Co., Ltd., azide equivalent is 247 g / mol;
[0040] 2 Purchased from Stai Chemical, flexible silicone resin, carboxyl equivalent weight is 2050 g / mol;
[0041] 3 Purchased from Beijing Bailingwei Technology Co., Ltd.;
[0042] 4Purchased from Hofmann Company of Germany, silica inorganic filler, high temperature resistant;
[0043] 5 Purchased from Beijing Bailingwei Technology Co., Ltd., chemically pure;
[0044] 6 Purchased from Clariant Chemicals, flame retardant;
[0045] 7 Purchased from BYK Chemical, dispersant;
[0046] 8 Purchased from Dow Chemical, high boiling point alcohol solvent;
[0047] 9,10 Purchased from Sinopharm Group.
[0048] The performance test results are shown in Table 2:
[0049] Table 2
[0050]
[0051] a Cut the material and inspect visually.
[0052] Embodiment 3-5
[0053] Example 3-5 relates to a method for synthesizing a heat-resistant and heat-insulating material, the composition and mass dosage of which are shown in Table 3 below:
[0054] Table 3
[0055]
[0056]
[0057] Remark: 11 Purchased from Shanghai Aladdin Reagent Co., Ltd., the azide equivalent is 205g / mol.
[0058] The performance test results of Examples 3-5 under the same test conditions are shown in Table 4 below:
[0059] Table 4
[0060]
[0061] The heat-resistant and heat-insulating material method involved in Example 6 and Comparative Example 1 has the following composition and mass dosage as shown in Table 5:
[0062] Table 5
[0063]
[0064]
[0065] Remark: 12 PPG Nouryon expandable microspheres.
[0066] The performance comparison between Comparative Example 1 and Example 6 is shown in Table 6 below:
[0067] Table 6
[0068]
[0069] In summary, the new heat-resistant and heat-insulating material of the present invention has excellent heat insulation and high temperature resistance after curing, and the temperature resistance of the material can reach 1300° C. It has excellent adhesion on the steel substrate.
[0070] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A temperature-resistant and heat-insulating material, It is characterized in that The material comprises the following components in terms of weight percentage of the total weight of the material: Other organic solvents are added to 100%; The molar equivalent ratio of the carboxyl group in the flexible silicone resin containing carboxyl functional groups to the molar equivalent ratio of the azide group in 3-(azidopropyl)triethoxysilane is 2:1-1.1:1; The palladium acetate (Pd(O 2 Ac) 2 ) accounts for 1-5% of the mass ratio of 3-(azidopropyl)silane.
2. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The 3-(azidopropyl)silane is at least one of 3-(azidopropyl)triethoxysilane and 3-(azidopropyl)trimethoxysilane.
3. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The flexible silicone resin containing carboxyl functional groups is a carboxyl-terminated flexible silicone resin.
4. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The mass ratio of the palladium acetate to 3-(azidopropyl)silane is 1-5%.
5. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The inorganic filler is a solid inorganic filler with a D50 particle size of 1 nm-100 μm.
6. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The mass ratio of the 4-dimethylaminopyridine to the 3-(azidopropyl)silane is 1-5%.
7. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The flame retardant is a liquid or solid flame retardant.
8. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The other additives are one or more combinations of dispersants, defoamers, wetting and leveling agents, and rheological additives; the other organic solvents include one or more combinations of esters, ketones, alkane solvents, and aromatic solvents.
9. The heat-resistant and heat-insulating material according to claim 1, It is characterized in that The high boiling point alcohol solvent is one or more combinations of polyethylene glycol, polypropylene glycol and dipropylene glycol.
10. Use of the heat-resistant and heat-insulating material according to any one of claims 1 to 9 in preparation, It is characterized in that It is applied on the substrate requiring heat insulation protection by spraying, dipping or brushing, and is formed into a film by thermal curing at 150-200°C.