High-strength low-modulus titanium alloy and high-frequency oscillation laser-induction composite additive manufacturing method thereof
The Ti-Nb-Cu-Mo alloy prepared by high-frequency oscillation laser-induction composite additive manufacturing method solves the problems of insufficient wear resistance and antibacterial properties of biomedical titanium alloy materials, and achieves high strength, low elastic modulus and Antibacterial properties improve the overall performance and preparation efficiency of the material.
Patent Information
- Application Number
- CN202410411855.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-08
AI Technical Summary
Existing biomedical titanium alloy materials have deficiencies in wear resistance and antibacterial properties, leading to implant infection and bone resorption problems. Traditional laser additive manufacturing technology has low preparation efficiency and has holes and crack defects in the material.
The Ti-Nb-Cu-Mo alloy is prepared using a high-frequency oscillation laser-induction composite additive manufacturing method. By adjusting the laser amplitude, frequency and scanning path, the lamellar α phase and strip-like α″ phase within the equiaxed β phase are formed. , and nano-Ti2Cu particles to achieve high strength, low elastic modulus and antibacterial properties.
A high-strength low-mode titanium alloy with high tensile strength, moderate elongation and excellent corrosion resistance was obtained, which reduced the temperature gradient of the molten pool and grain refinement, avoided pores and cracks, and improved the overall performance of the material.
Smart Images

Figure CN118308627B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomedical materials and additive manufacturing, and in particular relates to a high-strength low-modulus titanium alloy and a high-frequency oscillation laser-induction composite additive manufacturing method and application thereof. Background Art
[0002] Titanium alloys are considered to be ideal materials for orthopedic implants because of their low density, high strength, high corrosion resistance, complete inertness to the body environment, superior biocompatibility, and high connection ability with bones and other tissues. Currently, the most widely studied biomedical titanium alloy material is Ti-6Al-4V. However, the low wear resistance of Ti-6Al-4V alloy easily releases cytotoxic V elements, causing infection in patients. The success rate of revision surgery after infection is low, which will cause great pain to patients. In addition, the elastic modulus of Ti-6Al-4V alloy (100~120GPa) is higher than the elastic modulus of bone (0~30GPa), which easily causes a "stress barrier" effect, preventing stress from transferring to adjacent bones, thereby leading to bone resorption and bone cell death around them. In order to solve these problems, researchers have designed a variety of new titanium alloys for biomedical applications, such as Ti-35Nb-7Zr-5Ta, Ti-17Mo and Ti-30Zr-5Cr. These alloys mainly stabilize the body-centered cubic (bcc) structure of titanium alloys at room temperature by adding β-stabilizing elements (Ta, Nb, and Zr, etc.). Compared with Ti-6Al-4V alloy, these new β-type titanium alloys have a lower elastic modulus. However, their strength has decreased. Therefore, it is urgent to develop new β-type titanium alloys that meet the challenges and developments in the field of biomedical materials.
[0003] In addition, when titanium alloy is used as an orthopedic implant, it is easy to cause implant infection during surgery. When the infected implant is implanted into the human body, a serious rejection reaction will occur, resulting in implant failure. Therefore, it is necessary to develop titanium alloy implant materials with antibacterial properties. In recent years, studies have found that some metal ions (such as Cu 2+ 、Ag + and Zn 2+ Compared with antibiotics, bacteria will not have immune response to metal ions, which has good application prospects. However, after adding metal elements to make the alloy have antibacterial properties, the strength and corrosion resistance of the alloy are reduced to a certain extent.
[0004] Compared with traditional manufacturing technologies such as casting and forging, laser additive manufacturing technology can directly manufacture metal parts according to CAD solid models, and can realize free manufacturing of complex parts without molds. Therefore, laser additive manufacturing technology has received extensive attention and research in recent decades. However, the traditional laser additive manufacturing technology has low preparation efficiency, and the alloys produced have defects such as holes and cracks, which seriously reduce the comprehensive performance of the material.
[0005] Therefore, how to efficiently prepare biomedical β-titanium alloys that are closer to the elastic modulus of human hard tissue and at the same time have high strength, high corrosion resistance, low elastic modulus and antibacterial function has become one of the key technical problems to be solved by technicians in the fields of additive manufacturing and metal biomedical materials. Summary of the invention
[0006] In order to solve the deficiencies of the above-mentioned prior art, the present invention provides a high-strength low-modulus titanium alloy and a high-frequency oscillation laser-induction composite additive manufacturing method and application thereof. The high-strength low-modulus titanium alloy is mainly composed of an equiaxed β phase, in which lamellar α phase and strip-shaped α″ phase are distributed, and nano-Ti2Cu particles are randomly distributed at the grain boundaries. The lamellar α phase and strip-shaped α″ phase are distributed in the equiaxed β phase and are heterogeneous structures, playing a role of heterogeneous deformation induced strengthening; the nano-Ti2Cu particles are located at the grain boundaries of the equiaxed β phase, playing a role of dispersion strengthening and antibacterial. In addition, during the preparation process, by adjusting the laser amplitude, frequency, power and oscillation scanning path, pores and cracks can be eliminated, the temperature gradient of the molten pool can be reduced, and the grains can be refined. The Ti-Nb-Cu-Mo alloy provided by the present invention has excellent tensile strength, elongation, corrosion resistance, as well as antibacterial properties and low elastic modulus, and can be used as a high-comprehensive performance biomedical implant material, and has a very broad application prospect in the field of biomedical materials.
[0007] The first object of the present invention is to provide a high-strength and low-modulus titanium alloy.
[0008] The second object of the present invention is to provide a method for manufacturing high-strength and low-modulus titanium alloy by high-frequency oscillation laser-induction composite additive manufacturing.
[0009] The third object of the present invention is to provide an application method of high-strength low-modulus titanium alloy.
[0010] The first object of the present invention can be achieved by adopting the following technical solutions:
[0011] A high-strength low-modulus titanium alloy comprises a plurality of Ti-Nb-Cu-Mo alloys stacked in sequence, each of which is composed of an equiaxed β phase; a lamellar α phase and a strip-shaped α″ phase of a heterogeneous structure are distributed in the equiaxed β phase, and nano-Ti2Cu particles are randomly distributed at the grain boundaries; wherein the volume proportion of the components in the equiaxed β phase is: 2% to 4% for the lamellar α phase, 3% to 5% for the strip-shaped α″ phase, 1% to 3% for the nano-Ti2Cu particles, and the rest is the equiaxed β phase.
[0012] Furthermore, the average grain size of the equiaxed β phase is 25-38 μm, the average grain size of the lamellar α phase is 80-150 nm, the average grain size of the strip-like α″ phase is 70-120 nm, and the average grain size of the Ti2Cu particles is 15-40 nm.
[0013] The second object of the present invention can be achieved by adopting the following technical solutions:
[0014] A method for manufacturing a high-strength, low-modulus titanium alloy by high-frequency oscillation laser-induction composite additive manufacturing comprises the following steps:
[0015] S1: Place the Ti-Nb-Cu-Mo composite powder in a powder mixer for mechanical mixing, and then place it in a loading hopper of an automatic powder feeder after vacuum drying; wherein the chemical composition of the Ti-Nb-Cu-Mo composite powder is: Nb 30-35wt.%, Cu 1.0-7.0wt.%, Mo 1.0-4.0wt.%, and the balance is Ti, wherein the particle sizes of Ti, Cu and Nb are all 30-80μm, the particle size of Mo is 600-950nm, and the powder purity is higher than 99.9wt.%;
[0016] S2: adjusting the distance between the induction heating coil and the surface of the substrate so that the substrate can be heated effectively by the surface skin effect;
[0017] Position the laser beam and the powder nozzle of the automatic powder feeder in the induction heating zone to achieve the combination of the laser heat source and the induction heating source;
[0018] S3: Use a powder nozzle and argon gas to blow Ti-Nb-Cu-Mo composite powder into the molten pool formed by the composite heat source to prevent oxidation of the alloy powder during processing; use a high-frequency oscillation laser to control the stirring intensity of the laser beam in the molten pool and the oscillation path of the laser beam to adjust the flow direction of the molten pool, prevent the generation of bubbles in the molten pool during processing, and enhance the density and uniformity of the alloy;
[0019] S4: After the composite heat source is removed, the molten Ti-Nb-Cu-Mo powder rapidly solidifies and crystallizes on the substrate surface to form a single-pass Ti-Nb-Cu-Mo alloy, and then the CNC machine tool automatically moves in the vertical direction of the cladding speed according to the CAD model to form multiple passes of Ti-Nb-Cu-Mo alloy;
[0020] S5: After a layer of Ti-Nb-Cu-Mo alloy is composite-clad, the laser head, induction heating coil and powder nozzle return to the starting position of the current layer processing, and rise along the Z axis by the thickness of the current layer to clad the next layer of Ti-Nb-Cu-Mo alloy;
[0021] S6: repeat steps S3 to S5 until the size requirement of the Ti-Nb-Cu-Mo alloy is reached;
[0022] S7: heat treating the Ti-Nb-Cu-Mo alloy obtained in step S6 to obtain a high-strength and low-modulus titanium alloy, so as to achieve synergistic enhancement of strength, toughness, antibacterial properties and low modulus.
[0023] Furthermore, in step S2, the induction heating power is 30-100 kW, and the temperature of the substrate being induction heated is 300-800°C.
[0024] Furthermore, in step S3, the stirring intensity of the laser beam in the molten pool is controlled by adjusting the laser beam power, oscillation frequency, cladding speed and amplitude, wherein the laser beam power is 0.5~2kW, the composite cladding speed is 0.6~10m / min, the laser beam oscillation frequency is 500~2000Hz, and the laser beam amplitude is: -3~3mm in the X-axis direction and -3~3mm in the Y-axis direction.
[0025] Furthermore, in step S3, the flow direction of the molten pool is controlled by adjusting the laser beam oscillation path, and the shape of the laser beam scanning path is a straight line, a circle or a spiral.
[0026] Furthermore, before step S2, the substrate is ultrasonically cleaned with anhydrous ethanol and then dried in a vacuum drying oven.
[0027] Furthermore, the substrate is titanium or a titanium alloy.
[0028] Furthermore, the heat treatment step in step S7 is: subjecting the Ti-Nb-Cu-Mo alloy to a solid solution treatment at 900-950°C for 1-2h, then keeping it at 800-900°C for 1-2h, water cooling, and precipitating α″ in the alloy; then aging at 450-750°C for 1-3h, and then water cooling to obtain the α phase and the Ti2Cu phase.
[0029] The third object of the present invention can be achieved by adopting the following technical solutions:
[0030] A method for applying a high-strength low-modulus titanium alloy, and application of the high-strength low-modulus titanium alloy or the high-strength low-modulus titanium alloy prepared by the method in the field of biomedical materials.
[0031] Compared with the prior art, the present invention has the following beneficial technical effects:
[0032] 1. The high-strength and low-modulus titanium alloy (Ti-Nb-Cu-Mo alloy) provided by the present invention has a high content of β stabilizers (Nb, Cu and Mo), and belongs to a β-type titanium alloy. Compared with an α-type titanium alloy, it has a lower elastic modulus; Mo and Nb improve the corrosion resistance of the alloy; the lamellar α phase and the strip-shaped α″ phase located in the β phase present a heterogeneous structure, which plays a role of heterogeneous deformation-induced strengthening; the nano-Ti2Cu particles precipitated at the equiaxed β phase grain boundary play a role of dispersion strengthening and antibacterial effect;
[0033] 2. The method provided by the present invention can eliminate pores and cracks, reduce the temperature gradient of the molten pool, refine the grains, and prevent the generation of bubbles in the molten pool during processing, thereby enhancing the density and uniformity of the alloy by forming a composite heat source by high-frequency oscillation laser and inductive coupling, and adjusting the amplitude, power and oscillation scanning path of the laser beam to control the stirring intensity of the laser in the molten pool.
[0034] 3. The antibacterial rate of the Ti-Nb-Cu-Mo alloy provided by the present invention reaches 85-98%, the tensile strength is 0.8-1.0 GPa, the elongation is 10-20%, the elastic modulus is 50-90 GPa, and the corrosion rate is 0.25×10 -5 ~1.57×10 -5 mm / year. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0036] Figure 1 This is a schematic diagram of a linear oscillation trajectory of a laser beam according to Example 1 of the present invention;
[0037] Figure 2 A schematic diagram of the microstructure of the high-strength and low-modulus Ti-Nb-Cu-Mo alloy of Example 1 of the present invention;
[0038] Figure 3 A schematic diagram of a circular oscillation trajectory of a laser beam according to Embodiment 2 of the present invention;
[0039] Figure 4 A schematic diagram of a spiral oscillation trajectory of a laser beam according to Embodiment 3 of the present invention;
[0040] in, Figure 1 , 3 and in 4:
[0041] 1-oscillating laser beam, 2-linear oscillation track, 3-substrate, 4-induction heating coil, 5-circular oscillation track, 6-spiral oscillation track. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the present invention will be clearly and completely described in combination with the embodiments below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. It should be understood that the specific embodiments described are only used to explain the present application and are not used to limit the present application.
[0043] Embodiment 1:
[0044] With titanium plate as substrate, when the laser beam oscillation scanning path is a straight line (see Figure 1 ), the method for manufacturing high-strength low-modulus titanium alloy by high-frequency oscillation laser-induction composite additive manufacturing provided in this embodiment, the specific implementation steps are as follows:
[0045] (1) Select powder with a purity of more than 99.9%, and the content of each component of the alloy is: Nb30wt.%, Cu2wt.%, Mo2wt.%, and the balance is Ti;
[0046] (2) The powders weighed according to the mass ratio were mixed in a powder mixer for 3 h, and then placed in a vacuum drying oven and dried at 80 °C for 1 h;
[0047] (3) Clean the surface of the titanium substrate with anhydrous ethanol, then dry it in a vacuum drying oven set at 80°C for 2 h, and fix the dried substrate on the equipment forming table;
[0048] (4) Importing the pre-designed CAD 3D model into the computer processing program, and then slicing the CAD 3D model of the component to be formed to obtain a series of real-time high-frequency oscillation laser-induction composite cladding two-dimensional scanning trajectories;
[0049] (5) adjusting the distance between the induction heating coil and the surface of the substrate so that the substrate can be effectively heated by the surface skin effect; wherein the adjustment range of the distance between the heating coil and the surface of the substrate is 5 mm, the adjustment range of the induction heating power is 60 kW, and the temperature of the substrate being induction heated is 600°C;
[0050] (6) Position the laser beam and the powder nozzle of the automatic powder feeder in the induction heating zone to achieve the combination of the laser heat source and the induction heating source;
[0051] (7) Using argon gas, the Ti-Nb-Cu-Mo composite powder is blown into the molten pool formed by the composite heat source through a powder nozzle to prevent alloy oxidation during processing; the stirring intensity of the laser beam in the molten pool is regulated by adjusting the laser beam power, oscillation frequency and amplitude, and the flow direction of the molten pool is regulated by adjusting the laser beam scanning path; after the powder is stably blown in, high-frequency oscillation laser-induction composite cladding is started;
[0052] Among them, the laser power is 1.2kW, the composite cladding speed is 8m / min, and the laser beam oscillation frequency is 800Hz; the composite cladding direction is the X-axis direction, the lateral direction of the Ti-Nb-Cu-Mo composite material on the substrate surface is the Y-axis, and the direction perpendicular to the substrate surface is the Z-axis direction. The laser beam amplitude is: -3~3mm in the X-axis direction or -3~3mm in the Y-axis direction, and the laser beam oscillation path graph is a straight line (see Figure 1 );
[0053] (8) When the composite heat source is removed, the molten Ti-Nb-Cu-Mo composite powder solidifies and crystallizes quickly to form a single-pass Ti-Nb-Cu-Mo alloy. Then the CNC machine tool automatically moves in the vertical direction of the cladding speed according to the CAD model, and the moving distance is 70% of the width of the single-pass alloy.
[0054] (9) After a layer of alloy is oscillated and composite clad according to the CAD model, the laser head, induction heating coil and powder nozzle automatically return to the starting position of the current layer processing and rise along the Z axis to the thickness distance of the current layer;
[0055] The scanning direction is the composite cladding direction as the X-axis direction, the lateral direction of the Ti-Nb-Cu-Mo alloy on the substrate surface as the Y-axis direction, and the direction perpendicular to the substrate surface as the Z-axis direction;
[0056] (10) Repeat steps (7) to (9) until the requirements of the previously designed alloy CAD 3D model are met, and the work is completed;
[0057] (11) The formed Ti-Nb-Cu-Mo alloy was cut using a wire cutting machine, and the alloy was solution treated at 900°C for 2 h, then kept at 800°C for 2 h and water-cooled; the sample was then aged at 650°C for 2 h and then water-cooled. The treated sample was then subjected to phase, microstructure and composition analysis, followed by tensile strength testing, corrosion resistance testing and antibacterial performance testing.
[0058] The Ti-Nb-Cu-Mo titanium alloy after composite cladding using the above process parameters is equiaxed grain, see Figure 2 . The average grain size of the β phase is 27μm, the average grain size of the α″ phase is 81.2nm, the average grain size of the α phase is 84.5nm, and the average grain size of the Ti2Cu particles is 17.5nm. The alloy is composed of 90.7% equiaxed β phase, 4.4% strip-shaped α″ phase, 3.6% lamellar α phase and 1.3% nano-Ti2Cu particles. Among them, the hard lamellar α phase and the soft strip-shaped α″ phase in the equiaxed β phase present a heterogeneous structure, which plays a role of heterogeneous deformation induced strengthening; the nano-Ti2Cu particles located at the grain boundary of the equiaxed β phase play a role of dispersion strengthening and antibacterial.
[0059] After testing, the antibacterial rate of Ti-Nb-Cu-Mo titanium alloy reached 76.6%, the tensile strength was 0.84 GPa, the elongation was 18.5%, the elastic modulus was 55.8 GPa, and the corrosion rate was 0.98×10 -5 mm / year.
[0060] Embodiment 2:
[0061] When the laser beam oscillation path is circular (see Figure 3 ), the method for manufacturing high-strength low-modulus titanium alloy by high-frequency oscillation laser-induction composite additive manufacturing provided in this embodiment, the specific implementation steps are as follows:
[0062] (1) Select powder with a purity of more than 99.9%, and the content of each component of the alloy is: Nb32wt.%, Cu3wt.%, Mo1wt.%, and the balance is Ti;
[0063] (2) The powders weighed according to the mass ratio were mixed in a powder mixer for 3 h, and then placed in a vacuum drying oven and dried at 80 °C for 1 h;
[0064] (3) Clean the surface of the titanium substrate with anhydrous ethanol, then dry it in a vacuum drying oven set at 80°C for 2 h, and fix the dried substrate on the equipment forming table;
[0065] (4) Importing the pre-designed CAD 3D model into the computer processing program, and then slicing the CAD 3D model of the component to be formed to obtain a series of real-time high-frequency oscillation laser-induction composite cladding two-dimensional scanning trajectories;
[0066] (5) adjusting the distance between the induction heating coil and the surface of the substrate so that the substrate can be effectively heated by the skin effect; wherein the adjustment range of the distance between the heating coil and the surface of the substrate is 7 mm, the adjustment range of the induction heating power is 80 kW, and the temperature of the substrate being induction heated is 700°C;
[0067] (6) Position the laser beam and the powder nozzle of the automatic powder feeder in the induction heating zone to achieve the combination of the laser heat source and the induction heating source;
[0068] (7) Using argon gas, the Ti-Nb-Cu-Mo composite powder is blown into the molten pool formed by the composite heat source through a powder nozzle to prevent alloy oxidation during processing; the stirring intensity of the laser beam in the molten pool is regulated by adjusting the laser beam power, oscillation frequency and amplitude, and the flow direction of the molten pool is regulated by adjusting the laser beam scanning path; after the powder is stably blown in, high-frequency oscillation laser-induction composite cladding is started;
[0069] Among them, the laser power is 1.5kW, the composite cladding speed is 9m / min, and the laser beam oscillation frequency is 900Hz; the composite cladding direction is the X-axis direction, the lateral direction of the Ti-Nb-Cu-Mo composite material on the substrate surface is the Y-axis direction, and the direction perpendicular to the substrate surface is the Z-axis direction. The laser beam amplitude is: -4~4mm in the X-axis direction, -4~4mm in the Y-axis direction, and the laser beam oscillation path graph is a circle;
[0070] (8) When the composite heat source is removed, the molten Ti-Nb-Cu-Mo composite powder solidifies and crystallizes quickly to form a single-pass Ti-Nb-Cu-Mo alloy. Then the CNC machine tool automatically moves in the vertical direction of the cladding speed according to the CAD model, and the moving distance is 70% of the width of the single-pass alloy.
[0071] (9) After a layer of alloy is oscillated and composite clad according to the CAD model, the laser head, induction heating coil and powder nozzle automatically return to the starting position of the current layer processing and rise along the Z axis to the thickness distance of the current layer;
[0072] The scanning direction is the composite cladding direction as the X-axis direction, the lateral direction of the Ti-Nb-Cu-Mo alloy on the substrate surface as the Y-axis direction, and the direction perpendicular to the substrate surface as the Z-axis direction;
[0073] (10) Repeat steps (7) to (9) until the requirements of the previously designed alloy CAD 3D model are met, and the work is completed;
[0074] (11) The formed Ti-Nb-Cu-Mo alloy was cut using a wire cutting machine, and the alloy was solution treated at 900°C for 2 h, then kept at 850°C for 1.5 h and water-cooled; the sample was then aged at 700°C for 1.5 h and then water-cooled. The treated sample was then subjected to phase, microstructure and composition analysis, followed by tensile strength test, corrosion resistance test and antibacterial performance test.
[0075] The Ti-Nb-Cu-Mo titanium alloy after composite cladding using the above process parameters is equiaxed grain, see Figure 2 . The average grain size of the β phase is 31.25μm, the average grain size of the α″ phase is 94.7nm, the average grain size of the α phase is 98.5nm, and the average grain size of the Ti2Cu particles is 19nm. The alloy is composed of 89.6% equiaxed β phase, 4.6% strip-shaped α″ phase, 3.7% lamellar α phase and 2.1% nano-Ti2Cu particles. Compared with Example 1, more nano-Ti2Cu particles are precipitated at the grain boundaries of the equiaxed β phase in the alloy, giving the alloy higher strength and antibacterial properties.
[0076] After testing, the antibacterial rate of Ti-Nb-Cu-Mo titanium alloy reached 91.6%, the tensile strength was 0.89 GPa, the elongation was 15.2%, the elastic modulus was 59.6 GPa, and the corrosion rate was 1.06×10 -5 mm / year.
[0077] Embodiment 3:
[0078] With titanium plate as substrate, when the laser beam oscillation path is spiral (see Figure 4 ), the method for manufacturing high-strength low-modulus titanium alloy by high-frequency oscillation laser-induction composite additive manufacturing provided in this embodiment, the specific implementation steps are as follows:
[0079] (1) Select powder with a purity of more than 99.9%, and the content of each component of the alloy is: Nb35wt.%, Cu5wt.%, Mo4wt.%, and the balance is Ti;
[0080] (2) The powders weighed according to the mass ratio were mixed in a powder mixer for 3 h, and then placed in a vacuum drying oven and dried at 80 °C for 1 h;
[0081] (3) Clean the surface of the titanium substrate with anhydrous ethanol, then dry it in a vacuum drying oven set at 80°C for 2 h, and fix the dried substrate on the equipment forming table;
[0082] (4) Importing the pre-designed CAD 3D model into the computer processing program, and then slicing the CAD 3D model of the component to be formed to obtain a series of real-time high-frequency oscillation laser-induction composite cladding two-dimensional scanning trajectories;
[0083] (5) adjusting the distance between the induction heating coil and the surface of the substrate so that the substrate can be effectively heated by the skin effect; wherein the adjustment range of the distance between the heating coil and the surface of the substrate is 4 mm, the adjustment range of the induction heating power is 90 kW, and the temperature of the substrate being induction heated is 800°C;
[0084] (6) Position the laser beam and the powder nozzle of the automatic powder feeder in the induction heating zone to achieve the combination of the laser heat source and the induction heating source;
[0085] (7) Using argon gas, the Ti-Nb-Cu-Mo composite powder is blown into the molten pool formed by the composite heat source through a powder nozzle to prevent alloy oxidation during processing; the stirring intensity of the laser beam in the molten pool is regulated by adjusting the laser beam power, oscillation frequency and amplitude, and the flow direction of the molten pool is regulated by adjusting the laser beam scanning path; after the powder is stably blown in, high-frequency oscillation laser-induction composite cladding is started;
[0086] Among them, the laser power is 2kW, the composite cladding speed is 10m / min, and the laser beam oscillation frequency is 1000Hz; the composite cladding direction is the X-axis direction, the lateral direction of the Ti-Nb-Cu-Mo composite material on the substrate surface is the Y-axis direction, and the direction perpendicular to the substrate surface is the Z-axis direction. The laser beam amplitude is: -2~2mm in the X-axis direction, -2~2mm in the Y-axis direction, and the laser beam oscillation path graph is spiral;
[0087] (8) When the composite heat source is removed, the molten Ti-Nb-Cu-Mo composite powder solidifies and crystallizes quickly to form a single-pass Ti-Nb-Cu-Mo alloy. Then the CNC machine tool automatically moves in the vertical direction of the cladding speed according to the CAD model, and the moving distance is 50% of the width of the single-pass alloy.
[0088] (9) After a layer of alloy is oscillated and composite clad according to the CAD model, the laser head, induction heating coil and powder nozzle automatically return to the starting position of the current layer processing and rise along the Z axis to the thickness distance of the current layer;
[0089] The scanning direction is the composite cladding direction as the X-axis direction, the lateral direction of the Ti-Nb-Cu-Mo alloy on the substrate surface as the Y-axis direction, and the direction perpendicular to the substrate surface as the Z-axis direction;
[0090] (10) Repeat steps (7) to (9) until the requirements of the previously designed alloy CAD 3D model are met, and the work is completed;
[0091] (11) The formed Ti-Nb-Cu-Mo alloy was cut using a wire cutting machine, and the alloy was solution treated at 950°C for 2 h, then kept at 900°C for 2 h and water-cooled; the sample was then aged at 750°C for 2 h and then water-cooled. The treated sample was then subjected to phase, microstructure and composition analysis, followed by tensile strength test, corrosion resistance test and antibacterial performance test.
[0092] The Ti-Nb-Cu-Mo titanium alloy composite cladding using the above process parameters is equiaxed after cooling, see Figure 2 . The average grain size of the β phase is 33.14μm, the average grain size of the α″ phase is 103.2nm, the average grain size of the α phase is 105.7nm, and the average grain size of the Ti2Cu particles is 23.6nm. The alloy is composed of 88.3% equiaxed β phase, 5% strip α″ phase, 3.8% lamellar α phase and 2.9% nano Ti2Cu particles. Compared with Examples 1 and 2, the heterogeneous deformation-induced strengthening effect in the alloy is more significant, and more nano Ti2Cu particles are precipitated at the equiaxed β phase grain boundaries, giving the alloy higher strength and antibacterial properties, but the elongation will decrease. After testing, the antibacterial rate of the Ti-Nb-Cu-Mo titanium alloy reached 95.5%, the tensile strength was 0.96GPa, the elongation was 8.6%, the elastic modulus was 64.7GPa, and the corrosion rate was 1.51×10 -5 mm / year.
[0093] The above three embodiments obtain the above-mentioned Ti-Nb-Cu-Mo titanium alloys of different sizes and different proportions by changing the chemical composition of the Ti-Nb-Cu-Mo composite powder, the high-frequency oscillation laser-induction composite additive manufacturing process parameters and the heat treatment process parameters. More Ti-Nb-Cu-Mo titanium alloys of different sizes and different proportions can be obtained through more embodiments (chemical composition of different Ti-Nb-Cu-Mo composite powders, different high-frequency oscillation laser-induction composite additive manufacturing process parameters and heat treatment process parameters), which are not listed one by one in the embodiments of the present invention. The volume proportion of the components in the equiaxed β phase obtained through multiple experiments is: 2%~4% for lamellar α phase, 3%~5% for strip α″ phase, 1%~3% for nano Ti2Cu particles, and the rest is equiaxed β phase; the average grain size of the equiaxed β phase is 25~38μm, the average grain size of the lamellar α phase is 80~150nm, the average grain size of the strip α″ phase is 70~120nm, and the average grain size of the Ti2Cu particles is 15~40nm.
[0094] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high-strength, low-modulus titanium alloy, characterized in that: The high-strength low-modulus titanium alloy comprises a plurality of Ti-Nb-Cu-Mo alloys stacked in sequence, each of which is composed of an equiaxed β phase; the equiaxed β phase is distributed with a heterogeneous structure of lamellar α phase and strip α″ phase, which plays a role of heterogeneous deformation induced strengthening; nano Ti2Cu particles are randomly distributed at the grain boundaries of the equiaxed β phase, which plays a role of dispersion strengthening and antibacterial effect; Mo and Nb in the equiaxed β phase improve the corrosion resistance of the alloy; wherein the volume proportion of the components in the equiaxed β phase is: 2% to 4% for lamellar α phase, 3% to 5% for strip α″ phase, 1% to 3% for nano Ti2Cu particles, and the rest for equiaxed β phase; the antibacterial rate of the Ti-Nb-Cu-Mo alloy reaches 85 to 98%, the tensile strength is 0.8 to 1.0 GPa, the elongation is 10 to 20%, the elastic modulus is 50 to 90 GPa, and the corrosion rate is 0.25×10 -5 ~1.57×10 - 5 mm / year.
2. The high-strength, low-modulus titanium alloy according to claim 1, characterized in that: The average grain size of the equiaxed β phase is 25~38μm, the average grain size of the lamellar α phase is 80~150nm, the average grain size of the strip α″ phase is 70~120nm, and the average grain size of the Ti2Cu particles is 15~40nm.
3. A high-frequency oscillation laser-induction composite additive manufacturing method for a high-strength low-modulus titanium alloy as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1: Place the Ti-Nb-Cu-Mo composite powder in a powder mixer for mechanical mixing, and then place it in a loading hopper of an automatic powder feeder after vacuum drying; wherein the chemical composition of the Ti-Nb-Cu-Mo composite powder is: Nb 30-35wt.%, Cu 1.0-7.0wt.%, Mo 1.0-4.0wt.%, and the balance is Ti, wherein the particle sizes of Ti, Cu and Nb are all 30-80μm, the particle size of Mo is 600-950nm, and the powder purity is higher than 99.9wt.%; S2: Adjust the distance between the induction heating coil and the surface of the substrate so that the substrate can be effectively heated by the surface skin effect; Position the laser beam and the powder nozzle of the automatic powder feeder in the induction heating zone to achieve the combination of the laser heat source and the induction heating source; S3: Use a powder nozzle and argon gas to blow Ti-Nb-Cu-Mo composite powder into the molten pool formed by the composite heat source to prevent oxidation of the alloy powder during processing; use a high-frequency oscillation laser to control the stirring intensity of the laser beam in the molten pool and the oscillation path of the laser beam to adjust the flow direction of the molten pool and prevent the generation of bubbles in the molten pool during processing, so as to enhance the density and uniformity of the alloy; S4: After the composite heat source is removed, the molten Ti-Nb-Cu-Mo powder rapidly solidifies and crystallizes on the substrate surface to form a single-pass Ti-Nb-Cu-Mo alloy, and then the CNC machine tool automatically moves in the vertical direction of the cladding speed according to the CAD model to form multiple passes of Ti-Nb-Cu-Mo alloy; S5: After a layer of Ti-Nb-Cu-Mo alloy is composite-clad, the laser head, induction heating coil and powder nozzle return to the starting position of the current layer processing, and rise along the Z axis by the thickness of the current layer to clad the next layer of Ti-Nb-Cu-Mo alloy; S6: repeat steps S3 to S5 until the size requirement of the Ti-Nb-Cu-Mo alloy is reached; S7: heat treating the Ti-Nb-Cu-Mo alloy obtained in step S6 to obtain a high-strength and low-modulus titanium alloy, so as to achieve synergistic enhancement of strength, toughness, antibacterial properties and low modulus.
4. The method according to claim 3, characterized in that: In step S2, the induction heating power is 30-100 kW, and the temperature of the substrate being induction heated is 300-800°C.
5. The method according to claim 3, characterized in that: In step S3, the stirring intensity of the laser beam in the molten pool is controlled by adjusting the laser beam power, oscillation frequency, cladding speed and amplitude. The laser beam power is 0.5~2kW, the composite cladding speed is 0.6~10m / min, the laser beam oscillation frequency is 500~2000Hz, and the laser beam amplitude is: -3~3mm in the X-axis direction and -3~3mm in the Y-axis direction.
6. The method according to claim 3, characterized in that: In step S3, the flow direction of the molten pool is controlled by adjusting the laser beam oscillation path, and the shape of the laser beam scanning path is a straight line, a circle or a spiral.
7. The method according to any one of claims 3 to 6, characterized in that: Before step S2, the substrate is ultrasonically cleaned with anhydrous ethanol and then dried in a vacuum drying oven.
8. The method according to any one of claims 3 to 6, characterized in that: The substrate is titanium or titanium alloy.
9. The method according to any one of claims 3 to 6, characterized in that: The heat treatment step in step S7 is: subjecting the Ti-Nb-Cu-Mo alloy to a solid solution treatment at 900-950°C for 1-2 hours, then keeping it at 800-900°C for 1-2 hours, water cooling, and precipitating α″ in the alloy; then aging at 450-750°C for 1-3 hours, and then water cooling to obtain the α phase and the Ti2Cu phase.
10. An application method of high-strength low-modulus titanium alloy, characterized in that: Application of the high-strength, low-modulus titanium alloy according to any one of claims 1 to 2 or the high-strength, low-modulus titanium alloy prepared by the method according to any one of claims 3 to 9 in the field of biomedical materials.